On the Electric Conducting Power of Alloys .
By A. MATTHIESSEN , Ph. D. Communicated by Professor WHEATSTONE .
Received November 17 , -Read December 22 , 1859 .
THE method employed for the following determinations is described in the Philosophical Magazine ( February 1857 ) .
The precautions taken were the following:1 .
Almost all the wires were determined in naphtha ( rock-oil ) , and the temperature observed .
2 .
They were all soldered to two thick copper wires , whose resistances were known and brought into the calculations .
3 .
Two separate wires of each alloy , of different diameters , were generally pressed or drawn ( as it was thought possible that in pressing out the wires they might contain alloys of different compositions , as , for instance , when the amalgams are pressed , we find that at first almost pure mercury comes out of the small hole ) , and two determinations were made with wires cut from the first , and a third from the second wire .
4 .
The higher bismuth alloys were pressed in very fine wires , about 02 millim. diameter , in order to obtain concordant results* .
5 .
The diameters of the wires were measured at each end , and generally also in the middle ; pieces of the wire , after the resistance had been determined , being bent at the ends , so that they were at right angles to each other , and to the intermediate portion of the wire , in order that the diameter might be measured in two directions , which are also at right angles with each other , by laying the wire with its two ends vertical in succession .
The brittle wires were broken in short lengths , a number of them measured , and the mean taken of the values so found .
6 .
A number of normal wires of different lengths were used , so that when the resistances were great , equally accurate results could be obtained .
7 .
Those bismuth-alloys which expand on cooling , so much that the liquid metals break through the crust and form globules on the surface , were recast in small pieces , so that one whole piece was used for pressing the wire ; for it is very possible that the globules which form on the surface have a different contmposition from the part which first solidifies .
All the wires which were not pressed were hard drawn , and they were compared with a hard drawn pure silver wire , whose conducting power , taken at 0 ?
t , =100 .
To save space only the mean of the three determinations will be given ; the bismuth-tin series , however , is given in full , and serves as a fair specimen of the accuracy of the experiments ; and when no concordant results could be obtained , a mark ( + ) will be put to the alloy , and the value for its conducting power is , the mean of several determinations .
A greater accuracy than that which has been obtained could not be expected , on account of the great difficulty of pressing or drawing a wire perfectly round and of a homogeneous composition .
Those alloys which were drawn into wire will be underlined , and when the whole series was drawn , it will be mentioned in a foot note .
TABLE I. Bismuth-Tin Series .
Mean of Conducting TemperaConducting TemperaConducting TemperaAlloy .
power , ture .
power , ture .
power , ture .
Conduting TempeaI .
wire .
II .
wire .
III .
wire , power .
ture .
power .
ture .
Bi2o Sn ... ... ... 108 250 1 08 25'2 1-07 25-3 1]08 252 Bio9 Sn ... ... ... 0-420 270 0-414 27'2 0-421 27'2 0-418 27-1 Bi6 Sr ... ... ... 0-262 26-2 0-267 26-4 0-262 26-4 0-264 26-3 Bi44 Sn ... ... . .
0-246 26-7 0-244 26-9 0-244 26-9 0-245 26-8 Bi8o Sn ... ... . .
0-256 23-6 0-253 23-8 0-256 24-8 0'255 24-1 BilO Sn ... ... . .
0-352 24-4 0-357 24-8 0-360 24-8 0-356 24-7 Bi6 S. .
0-513 29-6 0-515 29-8 0-510 29-7 0-513 29-7 Bi4 Sn ... 0630 29-4 0-629 29-6 0-637 29-8 0'632 29-6 Bi2 Sn. .
1-03 30-0 1-02 29-9 1-06 29-9 1-04 29-4 Bi Sn ... ... ... 222 28-3 2-23 28-5 2-28 28-7 2-24 28-5 Bi Sn ... ... ... 3-93 25-6 3-97 25-7 3-97 25-8 3-96 25-7 Bi Sn4 ... ... . .
5-84 23-0 5-85 24-2 5-83 24-4 5-84 23-8 Bi St.6 ... ... .
7-02 27-8 7*12 28.0 6-99 28.0 7-04 27-9 Bi Sn8 ... ... ... 7-79 24-8 7-82 24-8 7-84 25-0 7-82 24-9 Bi Sn44 ... ... 10-22 240 10-43 24-4 10-57 24-3 10-41 24-2 Determinations made with pressed and drawn lead wires gave exactly the same values .
The following alloys , viz. the two last silver-lead , the two last silver-tin , the two last gold-tin , and all the goldand silver-copper alloys , were made in the manner which will be described in a paper " On the Conducting Powers of Copper , " &amp;c. , by Dr. M. HOLZMANN and myself .
The alloys used for the determinations were those whose specific gravities have been determined ; and the metals composing them may be classed under two heads , viz. Class A. Those metals which , when alloyed with one another , conduct electricity in the ratio of their relative volumes .
Class B. Those metals which , when alloyed with one of the metals belonging to Class A , or with one another , do not conduct electricity in the ratio of their relative volumes , but always in a lower degree than the mean of their volumes .
To Class A. belong lead , tin , zinc , and cadmium .
To Class B. belong bismuth , mercury , antimony , platinum , palladium , iron , aluminium , gold , copper , silver , and in all probability most of the other metals .
I shall now say a few words1 .
On the conducting power of the metals employed .
2 .
On the conducting power of the alloys made of the metals of Class A. with one another .
On that of alloys made of the metals of Class A. with those of Class B. 4 .
On that of alloys made of the metals of Class B. with each other .
5 .
General conclusions .
1 .
On the Conducting Power of the Metals employed .
They have all been redetermined , and the values found the same as those given in my paper " On the Electric Conducting Power of the Metals* , " with the exception of gold ( see Appendix at the end of this paper ) and copper ( " On the Electric Conducting Power of Copper , " &amp;c. ) .
These values are given in Table II .
TABLE II .
Specific gravities used for the calculation of Metal .
Conducting power .
Equivalent used .
the result .
10-468 Silver ... ... ... ... ... 100 at 0 108 8'921 t Copper ... ... ... . .
93'16 at 19-4 19-265 Gold ... ... ... ... ... 72-88 at 21-3 197 Aluminium ... ... ... 33-76 at 19*6 7'148 Zinc ... ... ... ... ... 27-39 at 17*6 32-6 8-655 Cadmium ... ... ... 2210 at 18-8 56-0 -Iron ?
... ... ... ... ... 14'14 at 20*4 -Palladium ... ... ... 12-64 at 17-2 7-294 Tin ... ... ... ... ... ... 1145 at 21-0 58 Platinum ... ... ... 10'53 at 20-7 11-376 Lead ... ... ... ... ... 7-77 at 19*3 103'7 6'713 Antimony ... ... ... 4-29 at 18-7 122-3 13-573 Mercury .
163 at 22'8 100 9'822 Bismuth ... ... ... ... 119 at 13-8 208 2 .
On the Conducting Power of the Alloys made of Metals belonging to Class A. with one another .
The mean of the three determinations found for the conducting power of these alloys is given in Table III .
, and also their calculated conducting powers , supposing that the conducting powers of the metals employed take part in that of the alloy in the ratio of their relative volumes 1 .
Lead-Tin Series .
Mean of Calculated conducting power from the Alloy .
Volume per cent. Conducting T. V D. power .
Temperatume .
Volume .
Diff. Pb Pb6 Sn ... ... ... ... ... ... 87'31 8-13 18-6 8'22 --009 Pb4 Sn ... ... ... ... ... 8 .
80 88 9'1 8'43 --015 Pb2 Sn ... ... ... ... . .
69-63 8-71 16-0 8'89 --018 Pb Sn ... ... ... ... ... ... 53-41 9'29 15-0 9-48 --019 Pb Sn2 ... ... ... ... ... ... 3643 10.15 15'9 10 ?
11 + 004 Pb Sn4 ... ... ... ... ... ... 2228 1057 16-2 10-63 -0 06 Pb Sn6 ... ... ... ... ... 16-04 10-78 18-6 10-86 --008o Tin-Cadmium Series .
Sn Sn6 Cd ... ... ... ... ... ... 88-06 12172 22-1 12-72 Sn4 Cd ... ... ... ... ... ... 83-10 13'23 22-3 13-25 --002 Sn2 Cd ... ... ... ... ... ... 71-08 14'44 20'2 14-53 -09 Sn Cd ... ... ... ... ... ... 55-14 16-14 20'9 16'23 -o09 Sn Cd2 ... ... ... ... ... ... 3806 18-36 19-6 18-05 +0'31 Sn Cd4 ... ... ... ... ... ... 2350 19 ' 62 20-3 19-60 -+002 Sn Cd6 ... ... ... ... ... ... 1700 20-42 20'5 20-29 +0-13 Tin-Zinc Series .
Sn Sn6 Zn ... ... ... ... ... ... 91-28 12-66 21-3 12-84 --018 Sn4 Zn ... ... ... ... ... ... 8746 13-32 20 '0 13-45 -014 Sn2 Zn ... ... ... ... ... . .
77-71 15-28 20-0 15-00 +0-28 Sn Zn ... ... ... ... ... ... 63-56 17-35 19'9 17-26 +0 09 Sn Zn2 ... ... ... ... ... . .
4658 19-67 21.1 19-96 -0-29 Sn Zn4 ... ... ... ... ... ... 30-36 22'28 20'1 22-55 -0'17 Cadmium-Zinc Series .
Cd Cd Zn ... ... ... ... ... ... 8949 22-48 19-4 22'65 -0-17 Cd4 Zn ... ... ... ... ... ... 85-02 22 ; 86 20-3 22-90 --010 Cd2 Zn ... ... ... ... ... ... 73-94 2345 21-3 23-48 --003 Cd Zn ... ... ... ... ... ... 58-66 23-87 22-3 24-29 -0-42 Cd Zn2 ... ... ... ... ... ... 41'50 24-13 22-2 25-19 -1-06 Cd Zn4 ... ... ... ... ... ... 2619 25-15 20-3 26-00 -0-85 Cd Zn ... ... ... ... ... ... 1912 2586 20.0 26-38 --052 Lead-Cadmium Series .
Pb Pb6 Cd ... ... ... ... ... ... 8943 838 21 9 9.29 -0-91 Pb4 Cd ... ... ... ... ... ... 84-93 8.99 23-0 9'93 --094 Pb2 Cd ... ... ... ... 73-81 10-20 18.5 11-52 --132 Pb Cd ... ... ... ... ... ... 58-49 12-61 21-8 13-72 --1-11 Pb Cd2 ... ... ... . .
4133 14.63 21-2 16-18 -155 Pb Cd4 ... ... ... ... . .
2605 17-70 20-7 18-37 -0-67 Pb Cd6 ... ... ... ... 19-02 18-98 21-4 19-38 --040 _~* ... ... .
164 Although the values found for some of the alloys of cadmium-zinc and lead-cadmium do not agree exactly with their calculated conducting powers , yet we see from their curves which are drawn on Plate V.* , that they do not vary much from straight lines , and we shall see further on that we cannot group them with either of the other classes .
3 .
On the Conducting Power of Alloys made from the Metals belonging to Class A. with those of Class B. The values found for the alloys of this class are given in Table IV .
, together with their calculated conducting powers .
TABLE IV .
Bismuth-Lead Series .
Mean of Calculated conAlloy .
Volume per cent. ducting power from Conducting power .
Temperature .
the volume .
Bi Bi160 Pb ... ... ... ... ... 9973 0-904 25-8 1-208 Bil25 Pb ... ... ... ... ... 99-66 0-610 23-8 1-213 Bioo Pb ... ... ... ... ... 99-57 0-428 24-8 1.218 Bi85 Pb ... ... ... ... ... 99-50 0-310 25-6 1-223 Bi70 Pb ... ... ... ... 99-39 0-291 25-0 123 Bi , Pb ... ... ... ... ... 99-11 0-270 21-3 1.25 Bi30 Pb ... ... ... ... ... 98-59 0-261 22.9 1.28 Bi24 Pb ... ... ... ... ... 98-24 0.257 24-1 1-31 Bi2o Pb ... ... ... ... ... 97-89 0-271 240 1-33 Bi,4 Pb ... ... ... ... . .
97-01 0-289 23-9 1-39 Bil2 Pb ... ... ... ... .
96-54 0-303 23-5 1-42 BiLo Pb ... ... ... ... ... 95-87 0-313 21-3 1-46 Bi8 Pb ... ... ... ... ... 94-89 0-357 22.6 1-53 Bi6 Pb ... ... ... ... ... 93-31 0-405 21.5 1-63 Bi4 Pb ... ... ... ... ... 90-28 0-521 2000 1-83 Bi2 Pb ... ... ... ... . .
82-29 0-859 19-9 2-35 Bi Pb ... ... ... ... . .
6991 1-41 192 3-17 Bi Pb2 ... ... ... ... . .
53-74 2-09 22-2 423 Bi Pb4 ... ... ... ... ... 3674 2-87 22-5 5-35 Bi Pb6 ... ... ... ... ... 27-91 3-47 21-3 5-93 Bi Pbs ... ... ... ... ... 22-50 4-02 21-7 6-29 Bi Pb , o ... ... ... ... .
18-85 4-35 20-9 6-53 Bi Pb24 ... ... ... ... .
883 5-55 24-4 7-19 Bi Pb1 04.5 2-27 7503 24-0 7-62 Bi Pb~oo ... ... ... ... ... '7-0324.07.62 Antimony-Lead Series .
Sb Sb2 Pb ... ... ... ... ... ... 80-00 2-86 242 4-99 Sb Pb ... ... ... ... ... . .
66-67 3-31 26-3 5-45 Sb Pb2 ... ... ... ... ... ... 5000 393 23-4 6-03 Sb Pb4 ... ... ... ... ... 33-33 4-72 24-1 6-61 Sb Pb6 ... ... ..25-00 5.52 26-1 6-90 Sb Pbo ... ... ... ... ... ... 16-66 6.03 254 7-19 Sb Pb ... ... ... . .
9-09 6-64 25.5 7-45 Sb Pb ... ... ... ... ... ... 385 709 23-7 7-64 ( continued .
) Lead-Gold Series .
Mean of Calculated conAlloy .
Volume per cent. ducting power from Conducting power .
Temperature .
the volume .
Pb Pb2o Au ... ... ... ... ... ... 9469 5-84 25-4 11-23 Pbo Au ... ... ... ... ... ... 8991 431 23-0 14-34 Pbs Au ... ... ... ... ... ... 87-70 3-76 26-1 15-78 Pb6 Au ... ... ... ... ... ... 8425 2'83 19 ' 7 18-03 Pb4 Au ... ... ... ... ... ... 78-10 3-01 223 2204 Pb Au ... ... ... ... ... ... 6407 3-59 16-8 31-18 Lead-Silver Series .
Pb Pb5o Ag ... ... ... ... ... 9769 7'91 25-3 9-81 Pb20 Ag ... ... ... ... ... 9464 8s06 24-3 12-71 Pb8 Ag ... ... ... ... ... 8760 8-49 26-6 19-20 Pb4 Ag ... ... ... ... .
7794 898 261 28-11 Pb2 Ag ... ... 63-86 10-68 15'6 41-10 Pb Ag ... ... ... .
46-90 11-69 16-5 56-73 Pb Ag ... ... ... ... 3064 15'63 13-9 71-74 Pb and Ag ... ... ... ... 1-39 47-62 23-8 98-72 Pb and Ag ... . .
0-89 67-13 23-4 99-18 Bismuth-Tin Series .
Bi Bi20o Sn ... ... ... ... ... ... 99-81 1-08 252 121 Bioo Sn ... ... 99-58 0-418 27-1 1-23 Bi60 Sn ... ... ... ... ... ... 99-38 0-264 26-3 1-25 Bi44 Sn ... ... ... ... ... ... 9915 0-245 26'8 1-28 Bi,3 Sn ... ... ... ... ... 98-76 0'255 24-1 1-32 Bilo Sn ... ... ... ... ... 96-38 0-356 24-7 1-56 Bi6 Sn ... 94-11 0-513 29'7 1-79 Bi4 Sn ... ... 91-42 0-632 29-6 2-07 Bi2 Sn ... ... ... .
84-19 1-04 29'9 2'81 Bi Sn ... ... ... ... . .
770 2*24 28'5 3'99 Bi Sn2 ... ... ... ... ... 57-19 3-96 25-7 5'59 Bi Sn4 ... ... ... ... ... 40-05 5-84 2338 7-35 Bi Sn ... ... ... ... ... 30-81 7-04 27-9 8'29 Bi Sn ... ... ... ... ... 2504 7-82 24-9 8-89 Bi Sn44 ... ... ... ... ... 5-73 10-41 24-2 10'86 Antimony-Tin Series .
Sb Sb Sn4 ... ... ... ... ... ... 3642 607 20-7 884 Sb Sn6 ... ... ... ... ... . .
2763 6-56 20-4 9-47 Sb Sn+ ... 18-64 7'21 224 10-12 Sb Sn2 ... ... ... ... ... ... 10-28 7-70 27-4 10-71 Sb Sn40 ... ... ... ... ... ... 5-42 849 27'0 11-06 Sb Sn ... ... ... ... ... ... 24 962 25-7 11-29 Sb Sn200 ... ... ... ... ... ... 113 998 79 1137 ( continued .
) Tin-Gold Series .
Mean of Calculated conAlloy .
Volume per cent. ducting power Conducting power .
Temperature .
from the volume .
Sn .
SnD10 Au ... ... ... ... ... 9873 11-11 23'6 12-23 Sno0 Au ... ... ... ... .
95-89 997 23-8 13-98 Snrl Au ... ... ... ... ... 93-33 9-18 24-2 15-55 Sn12 Au ... ... ... ... . .
9032 776 19'8 17-40 Sn8 Au ... ... ... ... ... 8615 6-13 19.2 19'96 Sn6 Au ... ... ... ... . .
82-35 4-98 21-7 2230 Sn5 Au ... ... ... ... . .
7954 4'28 21-3 24-03 Sn4 Au ... ... ... ... ... 7567 512 22-3 26-41 Sn3 Au ... ... ... ... ... 70-00 8-86 21.0 2990 Sn2 Au ... ... ... ... .
60-87 14'27 181 ] 35-51 Sn Au ... ... ... . .
43-75 8'88 15'9 46-03 Sn Au ... ... ... ... 2800 5.18 15.0 55-72 Sn and Au .
2'11 13-12 21-4 71-58 Sn and Au ... ... ... ... 117 19'59 188 72-16 Tin-Silver Series .
Sn Snl , o0 Ag ... ... ... ... ... 99-28 11-37 21'9 12-08 Sn,0 Ag ... ... ... ... ... 97-47 11-46 20-3 13-69 Sn36 Ag ... ... ... ... . .
9652 11-46 20-3 14-53 Sn24 Ag ... ... ... ... ... 94-87 11-57 20-3 15-99 Sn,8 Ag ... ... ... ... ... 93'28 11-56 20'1 17-40 Sn Ag ... ... ... ... 9025 11-53 20'1 20-09 Sn6 Ag ... ... ... . .
82-23 12-23 23-3 27-19 Sn4 Ag ... ... ... ... ... 7551 12-58 19'8 33-14 Sn2 Ag ... ... ... ... ... 6066 14-35 20o6 46-29 Sn and Agt ... ... ... 201 23-95 20-6 98-22 Sn and Agt ... ... . .
093 35-71 20-7 99-17 Heree find some cuom rious the metals composing them ; results , viz. that some alloys conduct less than either of ' and on looking at Plate VI .
$ , on which the curves of the conducting powers of the alloys belonging to this class are represented , we see how rapidly the conducting power decreases on the one side of the curve with small per-centages of the other metal ; and if we follow it to the other side , we find how little the conducting power of the metal of Class A. is affected by large per-centages of the metal of Class B. To this fact I shall return when I come to the general conclusions .
The lead and tin alloys , with a large proportion of antimony , could not be made into wire , on account of their extreme brittleness and hardness .
The alloys of lead with a large proportion of gold were so excessively hard , brittle and infusible , that they could * The gold in these alloys was determined .
t The amount of silver in these alloys was determined .
+ On the same Plate , in order to show the decrement of the conducting power of the bismuth alloys , parts of the bismuth-lead and bismuth-tin curves are drawn on a scale in which silver is taken as 1000 .
167 ot be pressed ; even gold alloyed with 25 per cent. of lead could not be drawn ; it appears to be perfectly rotten .
Most of the gold-lead alloys which were determined were much more brittle than glass .
The gold-tin alloys , although just fusible enough to press , were yet excessively brittle .
Silver with lead and tin could only be pressed or drawn within certain limits ; and where no wires could be obtained , that portion of the curve is denoted by dotted lines .
Nearly all the gold alloys , especially those rich in gold , were made with gold which had been precipitated by algaroth powder , &amp;c. ( see Appendix ) .
In Table V. are given some experiments made with certain commercial metals alloyed with pure tin or lead .
The values are the mean of two determinations ; and from the values found we see that they all belong to Class B , as they all conduct less than the calculated values .
TABLE V. Mean of Conducting power .
Temperature .
Hg Sn ... ... ... ... ... ... ... ... ... ... ... 378 220 Pb alloyed with 10 per cent. Pd ... ... 622 245 Sn alloyed with 10 per cent. Pd ... ... 906 24'2 Pb alloyed with 10 per cent. Pt ... ... 518 21*4 Sn alloyed with 10 per cent. Pt 9 ... .
9'37 21.1 Sn alloyed with 2'5 per cent. Fe* 9'71 20.5 Zn alloyed with 10 per cent. Al ... ... ' 24'02 24*5 *~ - .
v..I ... ... ... ... ... ... ... , ... ... ... .
, ... .
4 On the Conducting Power of Alloys made of the Metals of Class B. with one another .
The values found for these alloys are given in Table VI .
, and their curves on Plate V. TABLE VI .
Bismuth-Gold Series .
Mean of Calculated conAlloy .
Volume per cent.ducting power. .
| Conducting power .
Temperature .
from the volume .
Bi Bi90 Au ... ... ... ... ... .
99-47 101 240 1.57 Bi40 Au ... 9881 0'998 21.6 2.04 Bi20 Au ... ... ... ... ... ... 9764 1-09 19'9 2'88 Bi8 Au 94.31 1-25 21.9 5 ' 27 Bi4 Au,.,89 23 1-42 22.6 8.92 Bi2 Au ... ... ... ... ... 8055 182 13-7 15-14 Bi Au ... ... ... ... ... ... 6743 295 14-3 24-55 ( continued .
) Bismuth-Silver Series .
M Mean of ?
Calculated conAlloy .
Volume per cent. .
ducting power Conducting power .
Temperature .
from the volume .
Bi BiN2M Ag ... ... ... ... ... 9976 1.12 21-3 1043 Bi50 Ag ... ... ... ... ... ? ?
9904 1.11 21-4 2-14 Bi24 Ag ... ... ... ... ... 98-01 1-14 21-4 3.16 Bi12 Ag ... ... ... ... ... 96-10 1-32 19'9 5.05 Bi6 Ag ... ... ... ... ... 9249 1.65 21-6 8-61 Bi4 Ag ... ... ... ... .
89-15 1-78 20-3 I 11-92 Bi Ag ... ... ... ... 80-4 2-45 01 20-54 Bi Ag ... ... ... ... ... 67-23 3-30 21.4 33-56 Bi Ag2 ... ... ... ... 50-64 4-66 22-4 49-95 Bi Ag4 ... ... ... ... ... 3391 8.08 20.3 66-49 Bi and Ag ... ... ... ... 2-33 47-87 22-9 97-70 * The amount of silver was determined .
Gold-Copper Series .
''t Au Au and Cu ... ... ... ... . .
97-72 46-66 19'1 73-34 Au and Cu ... ... ... ..9 ... .
9567 33-01 19-4 73-75 Au and Cu ... ... ... ... ... 91-54 22.45 17-9 74-58 Au and Cu ... ... ... ... ... 83-83 15-35 20-3 76-16 Au and Cu ... ... ... ... ... 73-15 12.66 19.6 78-32 : Au and Cu ... ... ... ... ... 53-20 11'45 17-8 82'37 Au and Cu ... ... ... ... ... 38'05 12'49 20'1 85-44 Au and Cu ... ... ... ... ... 31'07 14-00 17-1 86-91 Au and Cu ... ... ... ... ... 19-36 19'86 16-9 89-23 i Au and Cu ... ... ... ... ... 11'43 28-74 I 195 90-84 Au and Cu ... ... ... ... ... 9-06 33-16 17-0 91-32 Au and Cu ... ... ... ... ... 3-53 53'18 18'0 92'44 Au and Cu ... ... ... ... . .
1-64 65-36 18'1 92-82 All hard drawn ; the amount of gold was determined .
Gold-Silver Series .
Au Au4 Ag ... ... ... .
98-81 59-09 25'1 73'25 Au6 Ag ... ... ... ... 98-'3 53-24 25-7 73-41 Au6 Ag ... ... ... ... ... ... 977 48-86 259 73-67 Au Ag ... ... ... ... ... ... 94-07 38-12 26-4 74-54 Au1 Ag ... ... ... ... ... ... 88-80 28-58 26-6 75-96 Au6 Ag ... ... ... ... ... ... 85-61 24'99 21.5 76-83 Au4 Ag ... ... ... ... ... ... .
79-86 20-91 21-0 78-38 Au2 Ag ... ... ... ... ... ... 66-47 16-20 20.2 82-01 Au Ag ... ... ... ... ... ... 49-78 14-59 22.2 86-52 Au Ag2 ... ... ... ... ... 33-14 16-30 19-9 91-03 Au Ag4 ... ... ... ... ... 19-86 20-94 21-2 94-62 Au Ag ... ... ... ... ... 14-18 1 25-29 19-9 96-16 Au Ag ... ... ... ... ... 11-02 9-87 19 9702 Au Ag ... ... ... ... ... 584 4119 0-5 98'4 Au Ag36 ... ... ... ... ... .
68 56-54 23-8 99'27 Au Ag5 ... ... ... ... . .
1-74 60-63 21-9 99-58 Au Ag4 ... ... ... ... ... 1:17 73-85 22-1 99-68 All hard drawn , not analysed .
169 2A ( continued .
) Copper-Silver Series .
Mean of Calculated conAlloy .
Volume per cent. -ducting power Conducting power .
Temperature .
from the volume .
Cu Cu and Ag ... ... ... ... ... 98-96 86-91 20'7 93-23 Cu and Ag ... ... ... ... ... 97-94 79-38 19'7 93-30 Cu and Ag ... ... ... ... ... 94-84 75-64 20'0 93-51 Cu and Ag ... ... ... ... ... 89-83 69-92 21'1 93-86 Cu and Ag ... ... ... ... ... 78-33 67-82 18-8 94-64 Cu and Ag ... ... ... ... ... 67-45 67-90 19'0 95-38 Cu and Ag ... ... ... ... ... 63-29 68-16 22'2 95-67 Cu and Ag ... ... ... ... . .
45-37 67-43 19'0 96-89 Cu and Ag ... ... ... ... ... 38-87 64-94 19-6 97-34 Cu and Ag ... ... ... ... ... 28-21 63-71 17-2 98-07 Cu and Ag ... ... ... ... ... 17-84 63'71 17'0 98'74 Cu and Ag ... ... ... ... ... 13-15 67'44 17-5 99'10 Cu and Ag ... ... ... ... ... 6-12 74-48 16-8 99-58 Cu and Ag ... ... ... ... ... 3-23 78-23 17-1 99-78 Cu and Ag ... ... ... ... . .
2.01 83-87 17-0 99-86 All hard drawn , and the silver determined .
Of the bismuth-gold alloys very few could be determined , as bismuth makes gold exceedingly brittle .
Gold could not be drawn with 025 per cent. of bismuth .
With silverbismuth , however , better results were obtained .
The bismuth-antimony alloys were determined , but as no concordant results were obtained , they will not be given ; the curve , however , appeared to be similar to those of this class .
On looking at the gold-silver alloys , we find that Au Ag conducts 14-59 ; Au , Ag and Ag2 Au conduct respectively 16-20 and 16-30 ; Au4 Ag and Ag4 Au conduct respectively 20'91 and 20-94 ; Au6 Ag and Ag6 Au conduct respectively 24 99 and 25 29 ; and from these points the difference becomes greater as we approach the pure metals .
But as 1 equivalent of gold =19725 =10226 volumes , and 1 equivalent of silver 108 =YO^68 =10317 volumes , we may regard the alloy Au Ag as being composed of 1 volume of gold+l volume of silver ; and within the above limits we may add to the alloy Au Ag equal amounts of gold or silver and obtain the same conducting power , showing that gold and silver within these limits , when alloyed with one another , have the same conducting power .
The same remarks hold good for some gold and copper alloys .
The curves of the alloys of this class show that there is a rapid decrement on both sides , of which I shall speak shortly .
170 General Conclusions .
The question now arises , What are alloys 1 Are they chemical combinations , or a solution of one metal in another , or mechanical mixtures 1 And to what is the rapid decrement in the conducting power in many cases due t To the first of these questions I think we may answer , that most alloys are merely a solution of the one metal in the other ; that only in a few cases we may assume chemical combinations , for example , in some of the gold-tin and gold-lead alloys ; and we may regard as mechanical mixtures some of the silver-copper and bismuth-zinc alloys .
The reasons of the foregoing assumptions are the following:1 .
That if we had to deal with chemical combinations , we should not find in the conducting power of alloys that regularity in the curves which certainly exists ; for on looking at those belonging to the different classes , we see at a glance that each class of alloys has a curve of a distinct and separate form .
Thus for the first , we have nearly a straight line ; for the second , the conducting power always decreases rapidly on the side of the metal belonging to Class B , and then turning , goes almost in a straight line to the side of the metal belonging to Class A. For the third group , we find a rapid decrement on both sides of the curve , and the turning-points united by almost a straight line .
If we now examine the part of the curve where the rapid decrement takes place , we find that in the lead and tin alloys it generally requires twice as much of the former as it does of the latter to reduce a metal belonging to Class B. to a certain conducting power ; for instance , to reduce that of silver to 67 , it would require 0-9 vol. per cent. of lead , or about 0-5 vol. per cent. of tin ; to reduce it to 47-6 , there would be required 1X4 vol. per cent. of lead , or about 0-7 vol. per cent. of tin .
Again , to reduce bismuth to -0261 , there is required 1-4 vol. per cent. of lead , or 0-62 vol. per cent. of tin ; and to reduce it to the minimum point of the curve , which is , when alloyed with lead , 0-255 , and 0-245 when alloyed with tin , it requires 1-76 vol. per cent. of lead and 0-85 vol. per cent. of tin .
2 .
We cannot explain the reason of the decrement of the conducting powers by assuming that the turning-points of the curves are chemical combinations , for it is not at all probable that there are such as contain only 06 per cent. of tin and 99-4 per cent. of bismuth ; or 2 per cent. of lead and 98 per cent. of bismuth ; or 2f6 per cent. of tin and 9-74 per cent. of silver , &amp;c. 3 .
That the alloys , at these turning-points , have their calculated specific gravities t. On Plate V. we find the curves of the alloys belonging to the third class : now here we might be inclined to think that we had to do with chemical combinations .
But if we consider , taking the gold-silver curve as a type , that the conducting power of silver is greatly reduced by small per-centages of any metal , and that the same may be said of gold , and if we suppose that this decrement has taken place , and join the two turningpoints to which the metals have been reduced , we shall have the gold-silver curve .
Take , x These values were read off from the curves .
t See the specific gravities of lead-bismuth and tin-bismuth alloys in this volume , pp. 162 , 165 , 166 .
2 A2 171 for instance , the gold-tin and the silver-tin curves , and connect the two turning-points , and we shall find that the curve so made is exactly similar to that of the gold-silver .
Again , look at that of the silver-bismuth , and compare it in the same manner with the tin-silver and tin-bismuth curves , and we obtain similar results .
The gold-bismuth and silver-bismuth curves are exactly similar ; the alloys of gold and bismuth conducting less than those of silver and bismuth , as would be expected , as silver is a better conductor than gold .
From the similarity of the curves of alloys , where we may assume , from their chemical behaviour , that we have only a solution of one metal in another , we may always draw approximatively the curve of the alloys of any two metals , if we know to which class they belong .
Thus before a single copper-gold alloy had been determined , the curve was almost correctly drawn , and agreed with that which was afterwards found by experiment .
That some alloys are chemical combinations may be deduced from the following facts : 1 .
At the turning-points of the curve we generally find the alloys contract or expand .
2 .
There is no regular form of curve ( see those of gold-tin , gold-lead , and silvercopper ) , so that it cannot be a priori even approximatively represented .
3 .
At the turning-points the alloys contain large per-centages of each metal .
4* At the turning-points of the curves the alloys are different from each other in appearance ( crystalline form , &amp;c. ) .
Now let us for a moment examine the gold-tin curve , it being the only nearly complete one of this class , and starting from the tin side of it , we find a slow decrement in the conducting power to the alloy Sn5 Au ; then a slow increment to Sn2 Au , and from this point a slow decrement to Sn Au2 .
For reasons before given , no alloys could be determined between Sn Au2 and that containing 2*7 per cent. of tin , from which point the curve goes in a straight line to pure gold .
Starting again from the tin side of the curve , we may regard the alloys down to Sn5 Au as a solution of a chemical combination in a metal ; from Sn5 Au to Sn2 Au , and from Sn2 Au to Sn Au2 , as a solution of two chemical combinations in each other , as all of these points are connected with each other by straight lines ; and from Sn Au2 to the alloy containing 27 per cent. of tin , as a solution of a chemical combination in an alloy , and from this point to pure gold as a solution of a small quantity of tin in gold .
Now these turning-points contain , first , Sn5 Au , 60 per cent. ; second , Sn2 Au , 37 per cent. ; and third , SnAu2 , 13 per cent. of tin , which may very well be considered to be chemical combinations .
On looking at their specific gravities , we find that Sn5 Au has almost its calculated one , whereas Sn2 Au expands , and Sn Au2 contracts more than any other of the gold-tin alloys experimented with .
In their general appearance we see that Sn Au2 and Sn2 Au are not at all crystalline , and have a very glassy fracture ; but Sn5 Au is exceedingly crystalline , and always shows , on being broken , the cleavage plane of a crystal from one end of the piece to the other .
172 For the above reasons I think there can be no doubt that the irregularity of the gold-tin curve is due to chemical combination , and that the same may be said of the gold-lead curve .
That some alloys are mechanical mixtures , we know from facts determined by other experimenters ; thus , when we fuse 17-73 parts of bismuth and 16*12 parts of zinc together , we find two layers , the upper one consisting of 13*40 parts of zinc , and the lower one 19*40 parts of bismuth alloyed with traces of zinc* ; now had we stirred the two metals well together , and cooled rapidly the alloy so obtained , it might be considered as a mechanical mixture .
Again , according to LEVOLt , if we fuse silver and copper together , and allow the alloy to remain quietly in the fused state , we find , on analysing the mass , that different parts contain different per-centages of metal : he found this to be the case with all alloys , excepting that containing 28f11 per cent. of copper , which corresponds to the formula Ag3 Cu4 .
LEVOL regards all alloys of silver and copper as mixtures of Ag3 Cu4 , and either silver or copper ; if this were the case , we should have expected to find from that point to pure silver or copper , straight lines ; but on examining that curve , starting from the copper side of it , we first see that a rapid decrement takes place , caused by the copper being alloyed with a small quantity of silver .
From that alloy containing 90 vols .
per cent. to that of 35 vols .
per cent. of copper , we have a straight line , and we may regard the intermediate alloys as mixtures or solutions of these two alloys ; from the alloy containing 35 vols .
per cent. to that with 28 vols .
per cent. of copper , we may have a mixture or solution of those alloys : now this last point is the minimum point of the curve , and corresponds almost to LEVOL'S Ag3 Cu4 , being an alloy containing 25 per cent. by weight of copper .
This , as well as the other lowest points of the curves , must not be considered as actually the lowest , but only as the lowest point found ; for in this case we should expect that the alloy containing 28 per cent. of copper would be lower ; and from this point to pure silver the alloys may be mixtures , or perhaps solutions of that alloy and silver containing a small quantity of copper .
Now it would appear as if at about the point which represents the alloy containing 35 vols .
per cent. of copper , there was also one of constant composition , otherwise we should have expected a straight line from the alloy containing 28 vols .
per cent. to that containing 90 vols .
per cent. of copper .
Of course , from this one curve , we can hardly deduce any conclusions , as we have in all probability to deal with mixtures of chemical compounds , with solutions of the one metal in the other , &amp;c. It only shows that , by the determination of the conducting powers of the alloys , we are able to tell where these are constant or chemical combinations ; and when the curves are irregular , we may safely conclude that we have to do with chemical combinations or mechanical mixtures .
That the first group of alloys , their curves being nearly straight lines , are not mix* FOURNET , Ann. de Chim .
et de Pliys .
, vol. liv .
p. 247 .
t Journ. de Pharm. , vol. xvii .
p. 111 .
173 tures but solutions of one metal in the other , may be deduced from the fact of their fusing-points being generally lower than the mean of that of the volumes taken .
Secondly .
To what is the rapid decrement of the conducting power due ?
The only answer which I can at present give to this question , is that most of the other physical properties of the metal are altered in a like manner ; for on looking at the alloys made with the metals of Class A. with one another , we see that most of their other physical properties are not at all altered ; for amongst them , for instance , we find no brittle ones ; they appear , in fact , to take an equal share of the properties of the metals composing them .
But now let us examine the alloys of the second class , and we immediately discover great differences ; alloy gold , the most ductile of all metals , with small per-centages of tin , lead , or zinc , and it becomes as brittle as glass .
Again , alloy silver with small per-centages of the above metals , and its properties are much altered .
Silver , which , when pure , is one of the easiest metals to draw , when alloyed with more than 3 per cent. of tin and 2 per cent. of lead , becomes so brittle , and its tenacity so much impaired , that it cannot be drawn .
I do not mean to say it is impossible to do so , but it was tried several times without success .
On the other hand , we do not find any marked differences in the ductility , hardness , &amp;c. of tin or lead when alloyed with silver ; we may add 10 , nay even 20 per cent. of silver to them , and they remain ductile , and may be pressed into wire without any trouble .
Of course , with lead and tin alloyed with small quantities of gold , the case is somewhat different , as we have here chemical combinations coming into play ; nevertheless , we may add to them 5 per cent. of gold without altering their ductility , &amp;c. to any great extent .
Bismuth alloyed with lead or tin becomes more brittle , and in wire its tenacity is impaired ; but tin and lead alloyed with large per-centages of bismuth , always retain a considerable amount of ductility , &amp;c. Again , take the alloys of the third class .
Although amongst the gold-silver and the gold-copper alloys we find no brittle ones , yet we know how hard gold , silver , and copper become when we alloy them with small quantities of other metals , and that they lose more in proportion of their ductility , &amp;c. , by the addition of small than of large quantities of strange metal .
From these facts , we need not be surprised at the rapid decrement of the conducting powers of the metals belonging to Class B , when alloyed with any other metal ; for when we find most of their other physical properties more or less greatly altered by traces of foreign metals , might we not also have expected this result For where we see no marked change in most of the other physical properties of alloys , as in the first class and in the second , on the one side of the curve , there we have nearly their calculated conducting powers .
It would be very interesting to determine quantitatively some of the other physical properties of the alloys , to see whether in them the tse properties will decrease in the same marked manner as the conducting powers , when a metal belonging to Class B. is alloyed with any other metal .
I intend therefore to commence , especially with this 174 view , with the conducting power for heat , in order to see if the classification of the metals and alloys given in this paper will hold good for any of the other physical properties , as well as in the hope of finding out the cause of the behaviour of the metals of Class B. when alloyed with traces of any other .
On looking at the specific gravity of alloys* , we find that they cannot be classified as above , but in all probability the above classification will hold good for their tenacity , hardness , conducting power for heat , &amp;c. APPENDIX .
On the Electric Conducting Power of Pure Gold .
The values given for the conducting power of pure gold , in my paper " On the Electric Conducting Power of the Metals t , " is not quite correct , as the gold from some cause cannot have been chemically pure ; although prepared with the greatest care by Dr. MEYBOOM , yet the wire-drawer in all probability fused it in a crucible which had been previously used ; and as only 3 to 4 grms. were purified , a very small amount of impurity would account for the difference which I have lately found .
At the time the values appeared very low , compared with those of other experimenters , but it was then thought that the higher ones were due to traces of silver .
Experiments , however , have proved , on the contrary , that most of the gold-silver , gold-copper , &amp;c. alloys conduct electricity worse than pure gold ; and that , in fact , only those which contain less than 2 per cent. gold in gold-silver alloys , and about 3 per cent. gold in gold-copper alloys , conduct better than pure gold .
Thus chemically-pure gold , prepared by dissolving gold from the refiners in nitrohydrochloric acid , precipitating with algaroth powder , washing alternately with nitric and hydrochloric acids , redissolving in nitrohydrochloric acid , precipitating by sulphurous acid , washing alternately with nitric and hydrochloric acids , and fusing in a muffle with nitrate of potash , gave , compared with a hard drawn silver wire =100 at 0 ?
C. , I. II .
III .
Mean .
73-57 at 190 ?
0 72-10 at 19 ?
-1 72-37 at 19 ?
*8 72-68 at 19 ?
03 .
Another specimen , prepared in the same manner , gave I. II .
III .
Mean .
72-80 at 23 ?
00 73-42 at 23 ?
-8 73-02 at 23 ?
-1 73-08 at 23 ?
03 .
A third specimen , prepared by dissolving gold containing silver in nitrohydrochloric acid , evaporating to dryness with excess of hydrochloric acid , dissolving in about 500 times its weight of water$ and precipitating with protosulphate of iron , washing out all the iron with boiling hydrochloric acid , and fusing with nitrate of potash and a little borax , gaveI .
II .
Mean .
73-63 at 13 ?
05 72-90 at 14 ?
'2 73-27 at 13 ?
08 .
A fourth specimen , prepared exactly as the third , gaveI .
II .
Mean .
74-20 at 14 ?
08 73-78 at 15 ?
'5 73'99 at 15 ?
-1 .
The so-called proof-gold of the refiners gaveI .
II .
III 65-57 at 23 ?
01 64-25 at 23 ?
01 65-92 at 23 ?
1* .
In conclusion , I give a list of the determinations of gold as found by other experimenters , silver taken = 100:RIEsst .
LENzt .
ED .
BECQUEREL .
HARRIS+ ... DAVYt .
CIIERSTIEt .
59 58-5 64-9 66-6 67 73 MATTHIESSEN .
55-19 and 73-26 at 17 ?
08 .
On looking over these values , we find that all , except that of CHRISTIE , are too low , and the gold-silver alloys which correspond to these numbers are the alloys which contain 99-4 per cent. gold and 0-6 per cent. silver , conducting 59 , 99-7 per cent. gold and 0'3 per cent. silver , conducting 66 .
Now the proof-gold of the refiners often contains as much as 05 per cent. silver , and the value 66 found for it would be that of the alloy 99-7 per cent. gold and 03 per cent. silver .
Of course the value given in my paper " On the Thermo-electric Series , " for the thermo-electric number of pure gold , cannot be correct , as I used the same gold for those determinations and for those of the conducting power .
I am much indebted to Dr. M. HOLZMANN for the excellent manner in which he has carried out the greater part of the foregoing determinations .
gold , and be reduced during the process of fusion .
The following experiments prove this to be the case ; they were carried out in every respect in the same manner , and with the same care as those above , the only difference being in the concentration of the solution .
Thus gold containing silver was dissolved in nitrohydrochloric acid , evaporated to dryness with excess of hydrochloric acid , dissolved in a small quantity of water and precipitated by a concentrated solution of protosulphate of iron , washed alternately by boiling nitric and hydrochloric acids , redissolved in nitrohydrochloric acid , reprecipitated by protosulphate of iron , washed alternately with nitric and hydrochloric acids and fused with nitrate of potash , and then gave 66-57 at 22 ?
00 .
Another specimen , prepared by precipitating a concentrated solution of gold by protosulphate of iron , washing , &amp;c. , redissolving and precipitating by sulphurous acid , washing , &amp;c. , gaveI .
67-87 at 22 ?
'3 .
II .
67-78 at 22 ?
03 .
For all the above determinations , hard-drawn wires were used .
t GMELIN , vol. i. p. 289 .
+ Ann. de Chim .
et de Phys. iii .
17 , 242..176 f/ u. / 221 .
VMD CCQLX .
Ijulde V. 'I-~~~~~~~ !
t-i ' ; i l--r---i i _1-Li-i I1-{i iL ii IL I~~~~~~~ rji I~ ~ ~~:J N]- ; i--t:-Al~~~~~~~~~~~~~~~~~~~~~~-i-t_i l -INK--li N I----------~~~~~~~~~~~~~-i--i-~-i-I-i-FK-AN -'-i-I~~~~~~~~~~~i:~--_'-_e~--iIIiF II1I NJJN iI I~~~~I ~L___ --A-AI-AI-i HiI -ii ; r-l-t -:~~ i- ; ii !
60 66 70 75 80 85 90 Zoln,7 s ' per Ce6n &amp; , b J.1B3naoi i. ; '/ uom2c ^ , pPoer 6('t ; .
, Cdiuo .
20