On the Electric Conducting Power of the Metals .
BY AUGUSTUS MATTHIESSEN , Ph. D. Communicated by CHARLES WHEATSTONE , Esq. , F.B.S. Received November 20 , 1857 , -Read January 14 , 1858 .
REQUIRING for my research on thermoelectricity a great many metals , which were for the most part chemically pure , I thought it would be interesting to determine at the same time their electric conducting power .
The method used for these determinations was the same as that described in the Philosophical Magazine ( February 1857 ) , and the experiments were made in the Heidelberg Physical Laboratory under the direction of Professor KIRcHHOFF .
The values given in the following series are the results obtained with different wires of the same metal compared with silver , 100 at 0 ? .
ConductTemperature .
Mean of Temperature .
ing power .
conducting power .
C. Silver. .
100 at 0 100 0 Copper , No. 3. .
77-43 at 18 8 77-43 18 8 72-70 at 22-6 Copper , No. 2 .
71 43 at 2266 .
72-06 2216 f 55.16 at 21-6 Gold ... 5524 at 218 5519 21-8 55417 at 22-0j Sodium ... ... 37-43 21-7 f 33.44 at 19-2 ' Aluminium ... 33T75 at 19-4 33-76 19-6 3409 at 20OJ 30-36 at 24.0 ] Copper , No. 1. .
307O5 at 24-2 I* 3063 24@2 1 30 90 at 24-5 2 2741 at h7 4 ) Zinc ... 27-42 at 17-6. .
27-39 17-6 27-34 at 17.8J Magnesium ... ... 25-47 17.0 Calcium .
22-14 16-8 { 22.05 at 18.8 ) Cadmium .
22-09 at 18-8 .
22410 18-8 { 22)16 at 18P8J ConductTemperature .
Mean of Temperature .
ing power .
conducting power .
0 ~~~~~~~~~~~0 Potassium.20 85 20 4 Lithium.19 00 20-0 14.64 at 21 2 ' 14-46 at 21-2 Iron ... . .
14-68 at 19-0. .
14-44 20-4 14-33 at 19-0 14410 at 214J ( 12.60 at 17.0 ) Palladium. .
12-63 at 17-2. .
12-64 17'2 I12-69 at 17.4J 1139 at 21.0 ) Tin. .
11 40 at 21-0. .
1145 21 0 11-56 at 21 0 ( 1055 at 2041 Platinum ... t 10-46 at 20-8. .
10 53 20 7 t10-57 at 21 0J f 7.84 at 17-2 ) Lead .
773 at 17-2 .
7.77 17-3 7*74 at 174J f 7*73 at 20 0 ) Argentine. .
7-62 at 17-4. .
767 18 7 7-67 at 18.8J Strontium. .
671 20 0S 4*28 at 18 7 ) Antimony ... 4 30 at 18-7. .
4 29 18-7 ( 4 29 at 18.7J 5 1.64 at 22.8 ) Quicksilver. .
1-63 at 22-8. .
163 22-8 51 62 at 22.8 r118 at14-51 Bismuth. .
1 19 at 14-8 1419 13-8 1 21 at 12 0 L1-19 at 14-0 Alloy of 0 880 at 24 0 ) Bismuth 32 parts 0-883 at 24 0. .
0-884 24-0 Antimony 1 part ( 0-889 at 24 0J Alloy of 0.516 at 220 ) Bismuth 12 parts 0(536 at 22-0. .
0519 22-0 Tin 1 part ... 0'505 at 22.0J Conducting Temperature .
Mean of Temperature .
power .
O a. conducting power C. Alloy of Antimony 2 parts { 0412 at 25.0 } 0 413 25-0 Zinc 1 part .
0-414 at 25-0.01 0.0719 at 22-0 Graphite , No. 1 .
** 0.0667 at 22 0 .
0*0693 22-0 Graphite , No. 2 .
0.0436 at 22 0 .
0*0436 22 0 0( 0372 at 25.0 ) Gas-coke..4 0 0405 at 25-0. .
0 0386 25-0 ( 090383 at 25-0J 0.00370 at 22-0 Graphite , No. 3 0000420 at 2 0 } .
0 00395 22-0 ( 000217 at 26.2 BUNSEN'S battery-coke..4 0-00289 at 26-2. .
0-00246 26-2 ( 000233 at 26-2J 0.000742 at 20-0 ) Tellurium. .
0 000795 at 20 0. .
0 000777 19-6 ( 09000794 at 18-7J 0'00000118 at 20.0 Red phosphorus 0 00000128 at 200 } 000000123 20 0 For the determination of the conducting powers of these bodies , whose electric resistance was very great , a number of normal wires of different lengths were made , and by these means accurate results were obtained .
The conducting powers of potassium and sodium * are here given to make the series complete .
The alloys of bismuth-tin , bismuth-antimony , and antimony-zinc were determined in order to ascertain whether , as they give with other metals such strong thermoelectric currents , they might be more advantageously employed for thermoelectric batteries than those constructed of bismuth and antimony .
All the metals were the same as those used for my thermoelectric experiments , with the exception of cadmium , which was purified by my friend Mr. B. JEGEL .
Coppers Nos. 1 , 2 and 3 , were wires of commerce .
In No. 1 small quantities of lead , tin , zinc , and nickel were found by Mr. HERSCHEL , who was kind enough to analyse it .
The small conducting powers of this sort may be attributed , according to the opinion of Professor BUNSEN , to a trace of suboxide of copper probably contained in the same .
The values obtained for aluminium are nearly the same as those found by POGGENDORFFf and BUF4 .
Iron , Nos. 1 , 2 and 3 , were pianoforte wires .
These determinations , although higher than those found by nearly all of the earlier experimenters , are in accordance with the results lately made known by BUFF .
The wires of bismuth employed for these experiments were of a very small diameter ( 0-144 millim. and 0-185 millim. ) ; for when manipulating with thicker ones , very varying results were obtained , probably owing to the disposition of the crystals , as MATTEUCCIhas already observed .
In fact , twelve experiments made with such wires , when the conducting power varied from 1411 to 1-36 , gave as a mean 1-20 , which agrees pretty accurately with the number in the above series .
Graphite No. 1 is the so-called pure Ceylon , No. 3 the purified German , and No. 2a mixture of both , all used for making pencils .
The specimens were purified by BRODIE'S patent , and pressed by Mr. CARTMELL , to whom I am indebted for the same .
These , as well as the gas-coke and BUNSEN'S battery-coke , were shaped into thin rods by hand , and the ends coppered galvanoplastically .
To form the connexion in order to determine their conducting powers , one end stood in a cup of quicksilver , the other cup being formed by placing an india-rubber tubing over the other end , the latter cup being of course also filled with quicksilver .
As the rods were made by hand , the difference in the results of the same specimens is thus accounted for .
An interesting fact was now observed , viz. that in all the cokes and graphites the conducting power increased by heat .
Some experiments were made with gas-coke , and it was found that if at 0 ?
the conducting power equalled 100 , it , from 0 ?
to 140 ?
, increased 0-00245 for each degree , and between the common temperature and a light red heat , about 12 per cent. For these experiments the connecting copper wires were soldered on to the coppered ends of the rods .
The red phosphorus was likewise coppered galvanoplastically , and the values determined after the same method .
The following metals were chemically pure:-Silver , gold , zinc , cadmium , tin , lead , antimony , quicksilver , bismuth , tellurium ; and the undermentioned pressed , viz. sodium , zinc , magnesium , calcium , cadmium , potassium , tin , lead , strontium , antimony , bismuth , alloy of bismuth-antimony , alloy of bismuth-tin , and tellurium .
No difficulty was found in pressing the above-mentioned wires , only with antimony and tellurium care must be taken in heating the press of the former to a dark red heat , and of the latter until it burns blue .
Quicksilver was determined in glass tubes , and the alloy of antimony-zinc cast likewise in small glass tubes , it being too hard to press and too brittle to draw .
The remainder of the wires were drawn .
In conclusion , I will record a few experiments on the alloys of lead , tin , zinc and cadmium .
The alloys made of two of these metals appear to conduct electricity after a very simple law ; namely , their conducting power is the mean of the conducting power of the quantity of each metal employed , as the following results show .
* Comptes Rendus , vol. xl .
p. 541 .
Mean of Mean of Calculated conducting power .
temperature .
conducting power .
0C .
SnPb* ... 920 21-4 9 09 Sn4Pb ... 10-55 22-0 10-31 Sn Pb4 ... 826 22-6 8-22 Zn Snt ... 17-43 22-0 17 13 ZnCd : ... 23-78 20 8 24-04 The above values are the means of at least two agreeing results determined after the before-mentioned method , the metals being of course chemically pure .
With bismuth and antimony the same law does not appear to hold good ; and how far with other metals this may be the case , I intend , as soon as I have procured a fresh supply of pure metals , to investigate and make known .