On the Constitution of the Resins .
By JAMES F. W. JOHNSTON , Esq. M.A. F.R.S. , Professor of Chemistry and Mineralogy in the University of Durham .
Received March 21 , -Read April 11 , 1839 .
THE object of the investigation , of which the present papel forms a part , is 1 .
To determine the relative composition of the various resins which occur in nature .
Possessing so many properties in common , this large family of natural produc.tions ought also to present many analogies in constitution .
2 .
To ascertain how far they may be considered as derivatives from one common radical ; and 3 .
Whether it is possible to represent them all by one or more general formulae .
I. Resin of Mastic .
Mastic resin is said to be obtained from the Pistacea lentiscus , and to be produced chiefly in the island of Chios .
It occurs in drops or tears , which are transparent , and of a pale yellow colour .
It melts at 212 ?
, and emits a peculiar and not unpleasant odour .
Fused in a retort it gives off an acid liquid in small quantity .
If the heat be raised to 300 ?
FAHR. and upwards , the melted mass froths up , and water and acid vapours are evolved .
At a higher temperature a pale yellow liquid distils over very slowly , at first of the consistence of oil , but increasing in thickness as the process proceeds , water and acid being also given off during the whole process .
What remains in the retort is of a black colour , and nearly insoluble in alcohol .
Digested in cold alcohol , mastic resin is in great part dissolved ; what remains is nearly pure white , elastic , capable of being drawn out into long fibres of a silky lustre , and is a compound with alcohol of a second resin ( B ) , very sparingly soluble in alcohol , but more largely in an alcoholic solution of resin A. Hence the solution obtained contains a portion of the second resin , which may be in a great measure precipitated by large dilution with alcohol .
I. The solution of resin A thus obtained is of a pale yellow colour .
Distilled and evaporated at 212 ?
FAHR. , it gives a pale yellow resin flowing freely at that temperature , but at higher temperatures frothing up and giving off alcohol .
Of a portion fused at 350 ?
FAHR. till it ceased to emit bubbles of vapour , 8'67 grains gave C= 24'685 , and H= 8818 10'73 grains gave C= 30'335 , and H= 9'80 10'294 grains gave C= 29-16 , and H= 9-614 These results give per cent. ( 1 .
) ( 2 .
) ( 3 .
) Carbon = 78'729 78*172 78'328 Hydrogen = 10'483 10'337 10-377 Oxygen = 10'788 11'491 11'295 100 100 100 These agree nearly with the formula C40 H32 04 , which gives Carbon -79275 Hydrogen = 10'355 Oxygen = 10-370 100 and was adopted by ROSE as representing the constitution of colophony .
The carbon , however , is deficient , and the hydrogen , according to the more recent analyses of TRONMMSDORF , LIEBIG , and LAURENT , is in larger quantity than in either the pinic or sylvic acid .
I therefore dissolved in alcohol a second portion of the mastic of the shops , diluted the solution largely* with alcohol to separate the resin B , evaporated and heated to 2600 FAHR. for eighteen hours , stirring it occasionally as long as bubbles of vapour were evolved in any quantity .
Of this resin 10 38 grains gave C= 29-785 , and H= 9'48 , or ( 4 .
) Carbon = 79'343 Hydrogen = 10'147 Oxygen = 10'510 100 which is almost identical with the result of ROSE for the crystallized resin of copaiva balsam .
II .
Heated again in the air to 350 ?
FAHR. it had lost its fragrant odour , and emitted white vapours .
In this state 8'718 grains gave C= 25'16 and H= 8'02 grains .
These are equivalent to ( 5 .
) C40 Ho3 04 gives Carbon = 79'800 79-79 Hydrogen = 10'221 9'77 Oxygen = 9'979 10'44 100'000 100'000 The carbon in this analysis is the exact theoretical quantity required by LIEBIG'S formula for the sylvic and pinic acids , but the hydrogen is still considerably in excess .
The resin thus analysed , however ( 5 .
) , had undergone a change of constitution by being heated to 330 ?
, for , when treated with alcohol , a large portion of it refused to dissolve , remaining behind as a soft reddish resin , on which the alcohol of the shops appeared to have little action in the cold .
After taking up all that was soluble , the alcoholic solution was evaporated , and the resin heated for two hours to 260 ?
FAHR. It was transparent , reddish yellow , and very beautiful .
On analysis 10'965 grains gave C= 31'925 H= 10*742 grains , which are equal to ( 6 .
) Carbon = 80'507 40 atoms Hydrogen = 10'885 = 33'11 atoms Oxygen = 8'608 = 3'27 atoms 100 The soluble part therefore of the changed resin was no longer pure mastic resin A ( see infra analysis , Nos. 26 , 27 , 28 .
) .
III .
A third portion of the mastic of the shops was boiled in water for several hours , by which it was rendered white , opake , and less fusible , probably from the loss of a portion of volatile oil existing in the resin of commerce .
It was then digested in a large quantity of alcohol , in which it now also dissolved more slowly .
The solution was evaporated , and the resin obtained again boiled in water for a length of time to drive off the whole of the alcohol .
1 .
A portion of this resin was then heated to about 2400 FAHR. , when it fused freely and ran smooth , and when cold had the same beautiful colour and appearance as that previously analysed .
10'956 grains gave C= 31'35 , and H= 10'136 , or per cent. ( 7 .
) Carbon = 79-122 Hydrogen = 10'279 Oxygen = 10'599 100 2 .
A second portion was heated only to 2120 for 48 hours , when it had become transparent and of a pale yellow colour .
At this temperature it softened , but did not enter into perfect fusion .
It still showed a tendency to form minute bubbles of gaseous matter .
10'713 grains gave C= 30'71 , and H= 10'02 grains , or per cent. ( 8 .
) Carbon = 79'265 Hydrogen = 10'392 Oxygen = 10'343 100 121 vDCCCXXXtX .
R The resin employed in these last analyses ( 7 .
and 8 .
) was entirely dissolved when treated with alcohol , No. 7 .
leaving only a trace of insoluble matter .
They may be considered therefore as representing very nearly the constitution of the soluble resin of mastic .
The formula C40 H31 04 agrees very closely with these results , and with that of analysis No. 4 , thus : ( 7 .
) ( 8 .
) ( 4 .
) Calculated .
Exper .
Exper .
Exper .
40 Carbon = 3057'480 = 79*531 79-122 79-265 79-343 31 Hydrogen = 386'867 = 10-063 10-279 10'392 10'147 4 Oxygen = 400-000 = 10'406 10'599 10'343 10-510 3844-347 100 100 100 100 If this be the true composition , it shows a close approximation to the pinic and sylvic acids , and yet a cause for the difference in the sensible properties exhibited by these different kinds of resin .
If such differences should actually be found to exist in nature , the striking fact will at once suggest itself , that under the general expression C40 132_- , 04 we may have a great variety of resins ; and a still greater variety , exhibiting also more sensible differences in their physical properties under the more general one of C40 H32_ x 04+y ' IV .
Action of Heat.-We have seen that when resin A is heated to 2600 FAHR. or upwards , it is partly decomposed , and an insoluble portion remains when it is treated largely with common alcohol in the cold .
This resin is in mass of a reddish colour , and is soluble in boiling alcohol , from which it falls as a yellow powder on cooling .
Dried at 212 ?
FAHR. it does not melt , but at about 130 ?
it begins to cohere into a dark reddish brown mass .
Heated for twelve hours at 212 ?
, and afterward exposed to a temperature at which it began to cohere , A. 8'538 grains gave C= 24-33 and H= 7-776 B. 10'994 grains gave C= 31'245 and -I = 9'976 These are equivalent to A. ( 9 .
) B. ( 10 .
) Carbon = 78'762 = 78'943 Iydrogen 10-119 = 10-128 Oxygen = 11119 = 10'929 100 100 2 .
As these results do not give any clear idea of what takes place when the resin is thus heated , I introduced a portion of the pure resin into a glass retort and kept it fused in a sand bath for twenty-four hours , the heat during the last twelve hours being raised to 270 ?
FAHR. Water was deposited in the neck of the retort , rendered sour by a crystallizable acid in small quantity .
The heat was withdrawn , when a 122 pale yellow liquid began to show itself in the upper part of the retort .
The resin was red and exceedingly beautiful , and when treated with alcohol was now separable into three portions .
A. Boiled with alcohol of the shops , a portion of a red colour was left , on which this liquid appeared to have little further action .
It adhered strongly to the retort , but was separated by boiling water , and obtained in the form of a dirty yellow powder , which , at 270 ?
FAHR. , showed no symptoms of fusion .
Dried at this temperature 8'475 grains gave C= 23'625 and H= 9-859 , or ( 11 .
) C40 H3o 05 gives C,0 H3 , O , gives Carbon = 77-080 77'76 77-51 Hydrogen 9-859 9'52 9-80 Oxygen = 13'061 12-72 12'69 100 100 100 From a single analysis , which was all that the quantity at my disposal enabled me to perform , it is impossible to determine which of the folrmulae represented in columns 2 and 3 is the true one .
Probability , however , is in favour of the first , or C40 H30 05 , which indicates that when decomposed by a moderate heat one of the changes which mastic resin A. undergoes is the substitution in a part of it , of an atom of oxygen for one of hydrogen , the new compound being nearly insoluble in common alcohol even at a boiling temperature .
B. The boiling alcoholic solution deposited on cooling a pale yellow , resin , which heated and fused , became brownish red .
11'817 grains gave C= 33'858 , and H= 10*356 grains .
C. The cold alcoholic solution , when evaporated and heated gently till perfectly transparent , gave a beautiful reddish yellow resin , of which 12'05 grains gave C= 34'003 , and H= 11'227 grains .
These results are equal to B. ( 12 .
) C. ( 13 .
) Carbon = 79'225 = 78'026 Hydrogen = 9'737 = 10'352 Oxygen = 11'038 = 11'622 100 100 From these analyses we cannot derive much information with regard to the constitution of these soluble portions of the changed resin , and it would be necessary to carry the process further than was done in this experiment , before the action of heat can be accurately understood .
If we might be guided in our opinions as to the ultimate nature of the soluble part by the constitution of the small quantity of which R2 123 No. 6 .
exhibits the analysis , we should infer that two new resins are produced , in the formulae for which are found 05 and 03 respectively .
But the subject requires further investigation , and I hope to be able to return to it at a future period .
V. Atomic weight of Resin A. It has been already observed by UNVERDORBEN that the resin of mastic bears a considerable resemblance to colophony , and combines with nearly the same proportion of oxide of lead .
A. Salts of Lead .
When a solution of this resin in alcohol is mixed with an alcoholic solution of acetate of lead , a white precipitate falls , which , when dried at 212 ?
becomes yellow ; at 350 ?
FAHR. it melts into a brownish yellow mass without decomposition .
1 .
Dried at 300 ?
FAHR. 1 1610 grains left 2-307 grains of oxide of lead = 19'878 per cent. 2 .
Of the samefused at 3500 FAHR. , 10-33 grains left 2-07 grains of oxide = 20-038 per cent. These give for the constitution of the salt 1 .
2 .
Resin ... 80-122 79-962 Oxide of lead .
19-878 20-038 100 100 It is therefore a sesquisalt =1 ( C40 H31 04 ) + Pb O , which consists of Resin = 80'527 1 Oxide = 19-4731 When boiled in alcohol , after being dried at 300 ?
FAHR. , this salt is not wholly dissolved .
Of that which was left undissolved in one experiment , 12'17 grains left 3-09 oxide of lead = 25-31 per cent. ] 8'805 grains left 2-20 oxide of lead = 24'99 per cent. in another experiment. .
( 15 .
) 8'57 grains left 2*232 oxide of lead = 26'04 per cent. 11'491 grains left 3-026 oxide of lead = 26'33 per cent. J These results agree with the formula ( C40 H31 04 ) + Pb O , which gives Resin = 73'388 1 Oxide = 26'612 J The boiling alcoholic solution deposits on cooling a white precipitate .
After being dried at 3000 , the portions of this precipitate obtained from the above two experiments were burned in the air .
A. 5'21 grains left 0-994 oxide of lead = 19'079 per cent. ] 5*52 grains left 1'044 oxide of lead = 18'913 per cent ... ( 16 .
) B. 9'217 grains left 1'683 oxide of lead = 18'249 per cent. J The salt thus precipitated is therefore the same as that obtained by the direct ac1-24 tion of the solutions of resin A. and of acetate of lead on each other .
When boiled on this sesquisalt , therefore , the alcohol decomposes it , dissolving a bisalt and leaving a neutral salt insoluble , while from the solution of the former a sesquisalt precipitates on cooling .
This accounts for a slight deficiency in the oxide of lead found in these salts ; the presence of a small quantity of a more acid salt in each causing a higher percentage of resin than is given by calculation .
When to the acid solution containing acetate of lead and resin A. from which this sesquisalt has been separated by filtration , pure ammonia is cautiously added with repeated agitation ; a further white precipitate falls , which is probably the neutral salt above described .
I did not dry this salt , but transferred it whilst still moist into boiling alcohol .
After repeated digestion a comparatively small portion only was dissolved , the boiling solution depositing the sesquisalt as it cooled .
The insoluble salt was collected and dried at 3000 FAHR. 5'93 grains left 2'452 of oxide of lead =41'357 per cent. It is therefore a disalt = ( C40 H31 04 ) +2 Pb 0 , which consists of By experiment .
Calculated .
Resin = 58'643 57-96 Oxide = 41'357 .
4204 ( 17 .
) 100 , 100 It appears , therefore , that resin A. of mastic forms with oxide of lead at least four compounds .
a. 2 ( C40 H31 04 ) + Pb 0 obtained in solution on boiling b in alcohol .
b. 3 ( C,4 H31 04 ) +2 Pb 0 by mixing the alcoholic solutions of the resin and of acetate of lead , and by subsidence from boiling solutions of a. c. ( C40 H31 04 ) + Pb 0 left insoluble when b is boiled in alcohol .
d. ( C40 H31 04 ) +2 Pb 0 left insoluble when the fresh precipitate from ammoniacal solutions of the resin and of acetate of lead is boiled in alcohol .
The compound a , as will appear from the preceding detail , is hypothetical , but its existence is necessary to explain the action of alcohol on the sesquisalt , and is rendered almost certain by the existence of an analogous silver salt* .
B. Salts of Silver .
When an ammoniacal solution of nitrate of silver in alcohol is poured into an alcoholic solution of mastic resin A , a pure white precipitate falls , soluble in large excess of ammonia , and becoming reddish brown in the sun 's rays .
Collected on the filter , and afterwards boiled with alcohol , it is nearly all dissolved , giving a slightly coloured solution , from which on cooling , a bulky white precipitate again falls .
This bulky precipitate was dried by pressure between folds of bibulous paper , and afterwards at a temperature of 250 ?
FAHR. Dried at 250 ?
, and still in the state of a white powder , it left 15*788 per cent. of metallic silver when burned in the air .
At 300 ?
, when it cohered , became of a dark colour , and gave a brownish red powder ; it left 16-042 per cent. of silver .
At 3500 FAHR. when it began to fuse it left 15'844 per cent. The mean of these three results is 15'891 per cent. of silver , or 17'066 of oxide of silver , therefore the salt consists of Resin ... 82'934 Oxide of silver =1 7066 e * ) 100 A compound represented by the formula 2 ( C40 1H31 04 ) + Ag 0 should contain 15'88 per cent. of oxide of silver , from which it would appear that the above is a bisalt with a small excess of silver .
That there are other salts of silver containing less acid is rendered probable by the difficulty of obtaining this bisalt without excess of base .
VI .
Constitution of the Resin Salts.-There remains still one important question to be solved in regard to the constitution of the salts of this and the other resins .
Does the resin unite with the oxide as a whole and without change , as muriatic acid unites with ammonia to form sal-ammoniac , or is it altered in any way , as the organic acids generally are when they combine with bases ?
Does it part with any of the oxygen or hydrogen it contains , when it forms a metallic salt ?
This inquiry is a very interesting one , and it is not at all answered by the experiments above detailed .
The results obtained are sufficiently wide of the quantities indicated by theory , to admit of considerable changes in the constitution of the resin , the existence of which can only be discovered by the ultimate analysis of the several compounds .
In the paper of ROSE on the constitution of colophony and some of the other resins * , the relative quantities of acids and base in several of the salts is investigated , but no ultimate analysis of them is given .
He only says , that , by the ultimate analysis of the salts , he obtained nearly the same composition for the resin as by analysing the pure resin itself .
From this it is fair to infer , that he found a slight difference , which he would naturally attribute to some impurity or imperfection in the salt employed , and would not , therefore , consider these results to be deserving of equal confidence with those obtained from the pure resin .
In the actual state of our knowledge in regard to the theory of the saline compounds of organic substances possessing acid properties , it would be a great step in advance were the constitution of the resinous salts accurately made out , and it might be expected to throw much light on the relative constitution of the different resins themselves .
Of the neutral salt of lead above described , 11 9 grains gave C= 25#14 , and H= 7'372 grains .
This is equal to ( 19 .
) Pb O+ ( C40 Hs , 04 ) gives Carbon. .
= 58'416 58'361 Hydrogen .
7'372 7-384 Oxygen. .
7'882 7-643 Oxide of lead 26-333 26'612 100 100 2 .
Of the sesquisalt of lead 2 Pb O+3 ( C40 H31 04 ) 1 128 grains gave C= 26'732 , and H= 8'446 grains .
This is equal to Experiment .
Calculated .
Carbon. .
= 65'529 64044 Hydrogen .
= 8'446 8-103 Oxygen. .
= 7'776 8379 Oxide of lead = 18-249 19'477 J 100 100 The first of these results is very near the theoretical constitution , and could it be exclusively depended upon , would indicate C40 H3o 04 as the formula for the resin .
The second analysis exhibits an excess of carbon , but the salt was not pure , as the quantity of lead it contained indicates .
Want of material prevented me from repeating the analysis .
Both results , however , are equally satisfactory in showing , that , in combining with the oxide of lead , the resin parts with none of its oxygen , and that the base does not replace any of the elements which it contains in an uncombined state .
3 .
Of the subsalt 2 Pb O+ ( C40 H31 04 ) dried at 300 ?
FAHR. A. 13'6 grains gave C= 22'54 , and H= 7'064 B. 14'11 grains gave C= 24'00 , and H= 7'127 C. 8'925 grains gave C= 14-77 , and H= 4-595 .
These are equal to A. ( 21 .
) B. ( 22 .
) C. ( 23 .
) Carbon. .
= 45'827 47'033 45-760 Hydrogen .
= 5-767 5'612 5'720 Oxide of lead = 41-355 41'355 41*355 Oxygen. .
= 7'049 5'998 7'165 100 100 100 The formula requires 40 Carbon. .
3057'48 = 46'09 31 Hydrogen .
= 386'86 = 5'86 2 Oxide of lead = 2788'99 = 42'04 4 Oxygen..= 400'00 = 6'01 6633'34 100 The second analysis B. exhibits a considerable excess of carbon , probably from an error of analysis .
All the three , however , agree in representing the hydrogen as less than the formula adopted for the resin requires .
A salt consisting of ( C40 H30 04 ) +2 Pb O would contain Carbon. .
= 46'16 Hydrogen .
= 5'65 Oxide of lead = 42-12 Oxygen .
= 607 100 The quantity of hydrogen is even sufficiently small to allow us to represent the resin by ( C40 H29 04 ) , while the neutral salt appears to contain ( C40 H30 04 ) .
We can draw no inference in regard to the amount of hydrogen it contains from the analysis of the sesquisalt , from its apparent impurity ; but in the other salts of lead the hydrogen present is manifestly less than in the pure resin according to the analyses above given ( 4 , 7 and 8 .
) .
Can the metal replace the hydrogen , giving in the one C40 H30 Pb1 05 , and in the other C40 HI29 Pb2 06 , and can such be the general constitution of the resin salts ?
This can only be determined by numerous and refined analyses of these compounds .
4 .
The salt of silver prepared , as already described , by precipitation and subsequent resolution in alcohol , and containing 16,954 per cent. of oxide of silver , gives a different result from those of lead in regard to the constitution of the resin .
A. 12-565 grains after heating to 3000 FAHR. , when it began to fuse , gave C= 30-74 , and H= 9-704 .
B. Heated to 250 ?
0only , 1'38 grains gave C= 28'293 , and H= 8-9 grains .
These results give per cent. A. ( 24 .
) B. ( 25 .
) Calculated .
Carbon ... = 67'595 68'673 68'589 Hydrogen. .
8'581 8'689 8'398 Oxygen ... = 6870 5'684 6-732 Oxide of silver 16-954 16'954 16'281 100 100 100 The third column is calculated according to the formula 2 ( C40 H30 03 ) + Ag 0 , and approximates as closely to the experimental results as was to be expected from a salt containing an excess of oxide , probably from the presence in small quantity of a less acid compound .
It appears , therefore , that in uniting with oxide of silver , the elements of an atom of water have been given off , the resin C40 H31 04 becoming C40 H30 03 +H O. And yet that this is not owing to a simple replacement of hydrogen by silver in the salt , is shown by its containing two equivalents of resin to one of oxide , 2HO being given off while Ag O only is taken up .
It is by no means clearly deducible from these 128 analyses , therefore , that the constitution of the resin of mastic A. is truly represented by C40 H30 03 + HI 0 , since during the treatment with silver and ammonia some deeper change may have been effected , giving rise to a new resin represented by C40 H30 03 .
And that this is really the case , seems to be confirmed by an examination/ of the anlmoniacal alcoholic solution from which the salt of silver has been precipitated .
When this solution is decanted , and by distillation is concentrated and deprived of its excess of ammonia , it becomes of a brown colour , and a dark brown resin falls to the bottom of the retort or of a jar , into which the solution may be poured .
On further concentration , after cooling , more of this resin falls , after which a precipitate of a white silver salt makes its appearance .
Separated by decantation , and kept for twelve hours at 212 ?
FAHR. , at which temperature it melted readily , A. 5'089 grains of this brown resin burned in the open air , left 0'85 of silver , equal to 1'786 per cent. of oxide .
B. 10-97 grains burned with oxide of copper , gave C= 3167 , and H 10*565 .
Correcting B by A , the resin consists of ( 26 .
) C40 Hs3 03 gives Carbon 81'280 81*385 Hlydrogen = 10'895 10*620 Oxygen = 7'852 7*995 100 100 When dissolved in alcolhol a small quantity of a dark brown silver salt was separated .
After filtration , evaporation , and fusing at 212 ?
for several hours , the resin was obtained nearly free from silver .
A. 3'061 grains left , when burned in the air , 0016 = 0'522 per cent. B. 9'158 grains gave C= 26'525 , and H= 9.0 .
C. After heating for several hours at 300 ?
FAHR. , during which a fragrant odour was emitted , 10*155 grains gave C= 29*40 , and H= 9.933 .
These gave for the constitution of the resin A ( 27 .
) B ( 28 .
) Carbon = 80 510 80'474 Hydrogen = 10*976 10'925 Oxygen = 8'514 8'601 100 100 If we admit , as is very probable , that the excess of hydrogen and oxygen indicated by these analyses .
over those obtained in analysis 26 .
is due to the presence of a small quantity of water , even after heating at 3000 FAHR. , the three results become entirely accordant* , and leave little doubt that the constitution of the resin is ex* The discordance in the results thus obtained for the same mass , of the same resin before and after solution MICCVXXXIX .
S 129 pressed at least very approximately by C40 H32 03 .
In looking back upon our previous analyses also , we find in No. 6 .
a very close agreement with these now given ; from which , compared with No. 11 .
, it would appear that by the long continued action of a temperature not below 350 ?
FAHR. the resin of mastic A , besides other alterations , is changed into a soluble resin containing three , and into an insoluble resin containing probablyfve equivalents of oxygen .
The constitution of the resin formed during the preparation of the silver salt , seems thus to confirm the opinion above stated , that a deeper change is produced upon resin A during the treatment with nitrate of silver and ammonia , than the simple extrication of the elements of an atom of water .
The large quantity of hydrogen present in the new resin especially supports this view .
In the silver salt we have taken C40 H30 03 as the most probable expression for the resin it contains , assuming , as is usually done , that the lowest amount of hydrogen obtained by analysis is greater than the truth .
In the analysis of the resin itself the same precautions were taken , yet C40 1I32 03 contains the lowest amount of hydrogen which the results permit us to adopt .
The presence of moisture in the oxide of copper could not , with the precautions adopted , occasion so great an excess of hydrogen ; and in analysis ( 26 .
) there is no corresponding excess of oxygen to justify us in attributing the difference to hygrometric water in the resin itself .
5 .
With the view of investigating more closely the action of oxide of silver on the resin A , I dissolved a portion of it in alcohol , added to the solution a little caustic ammonia , and afterwards an alcoholic solution of nitrate of silver .
The white salt which fell was collected on the filter , washed with cold alcohol , and afterwards dried at 300 ? .
It melts at a low temperature in the alcohol it retains , and is obtained in the form of a dark red porous mass .
By a careful regulation of the heat , however , it may be dried without undergoing fusion .
5'177 grains , burned in the air , gave 0*923 of metallic silver = 17*829 per cent. 4'404 grains gave 0'79 = 17'94 per cent. of silver , or 19*26 of oxide of silver .
11 632 grains gave with oxide of copper C= 26*87 , and H= 8'69 .
These results give for the composition of the salt ( 29 .
) In equivalents .
Carbon 63'87 = 40 Hydrogen = 830 = 31'8 Oxygen = 8'57 = 41 Oxide of silver = 19-26 = 06 100 in alcohol , is not without interest in a research into the general constitution of the resins .
It shows that , with all our precautions , small differences will occur from circumstances not yet understood , and that in our selection of a formula to represent the constitution of a given resin , we ought to allow analogy to influence us in some degree where the results of analysis are not sufficiently numerous and concordant unequivocally to settle the question .
To this point I shall have occasion to revert in a future paper on the constitution of certain other resins .
130 TRhe resin in this salt is evidently C4Q 13j 04 , or in combining with the silver by this method of preparation it undergoes no change .
There is present a considerable excess ( one-sixth of the whole ) of silver , probably from an admixture of a less acid salt .
After the separation of the salt thrown down as above , nitrate of silver was still added as long as a precipitate fell .
This second precipitate was collected and digested in boiling alcohol .
A transparent slightly brownish solution was obtained , from which on cooling a white compound fell , but at the same time a considerable portion of a dark brown resin or resinous salt was precipitated on the sides and bottom of the retort in which the solution was effected .
The white precipitate was collected and dried at 300 ?
FAHR. 4 167 grains left 0 64 of metallic silver = 15*36 per cent. , or 16,496 of oxide of silver .
A. 11'975 grains , burned with oxide of copper , gave C= 28'62 , and I= 9'195 .
B. 8*67 grains gave H= 6'703 , the carbonic acid being lost .
The salt therefore consists of A. ( 30 .
) B. 2 ( C40 H3 , 04 ) + Ag O gives Carbon = 66'086 66-79 Hydrogen = 8'530 8*59 8'46 Oxide of silver = 16-496 1588 Oxygen = 8'888 8-87 100 100 The bisalt of oxide of silver therefore , prepared without large excess of ammonia , is not decomposed by solution in pure alcohol , the change produced upon it and upon the resin in the former experiment being due either to the excess of ammonia or to the long boiling .
Still though the salt obtained in this instance contained the unchanged resin A , yet when the alcoholic solution from which the precipitates were originally thrown down , was concentrated by distillation , there fell , on allowing the solution to cool , first , a portion of a white precipitate , and afterwards , on still further concentration , a quantity of a dark coloured resin , closely resembling the C40 H32 03 , above described and analysed .
It appears therefore to be easily reproducible , though the circumstances necessary to its production require further investigation .
In regard to the hydrogen contained in this salt , the analysis seems to indicate thirty-one equivalents , which does not agree with the change undergone by the resin in combining with the oxide of lead .
It is not impossible , however , that the true formula for the salt may be Ag 0+ ( C40 H30 04 ) + ( C40 H31 04 ) , which would give 8-34 per cent. of hydrogen , a quantity not differing from 8-53 found by analysis , more than the ordinary results of experiment do from the calculated results ; but upon this subject I would not be understood to express a decided opinion until it has undergone further examination* .
Insoluble Resin of Mastic ( Resin B. ) .
When crude mastic resin is digested in cold alcohol a variable quantity remains undissolved .
This portion is soft , tenacious , and elastic like bird-lime , of a silky lustre , and may be boiled in alcohol without sensible diminution .
When boiled in water it becomes harder and less elastic ; but when deprived of water by drying at 300 ?
FAHR. , at which temperature it is in a semifused state , it may be drawn out into long fibres , and even when cold it is tough and has some of the elasticity of caoutchouc .
1 .
Burned in the open air it left a small gray residue of carbonate of lime , being earthy matter mixed with the natural resin .
6'358 grains left 0-06 = 0'945 per cent. 2 .
Burned with oxide of copper after drying at 300 ?
FAHR. A. 12'863 grains gave C= 38'624 , and HI = 12-645 .
B. 11605 grains gave C= 34'75 , and = 11.395 .
These results , allowing for the small quantity of foreign matter present ( 0 954 per cent. ) , are equivalent to ( 31 .
) ( 32 .
) Carbon = 83'823 = 83-589 Hydrogen = 11-027 = 11-013 Oxygen = 5'160 = 5'398 100 100 The formula which approaches nearest to these results is C40 H31 02 , giving 40 Carbon = 3057'480 = 83'613 31 Hydrogen = 399'347 = 10-920 2 Oxygen = 200'000 = 5-467 3656-827 100 The slight excess of carbon in the first analysis is probably due to some accidental cause .
It may have been from a greater admixture of foreign matter in the one portion than in the other , that the small difference has arisen .
When this resin is exposed to a higher temperature it swells , gives off the odour of naphtha ( ?
) , and the porous mass , when cold , is no longer soft but brittle .
Analysed in this state it gave the formula ( C40 i31 03 ) , but I did not ascertain how much foreign matter this specimen contained , and the coincidence of the result with this formula may be accidental .
This resin does not sensibly dissolve in a solution of caustic potash , it is , therefore , most probably not an acid resin .
VIII .
Conclusions .
In regard to the resin of mastic , it therefore appears , from the preceding examination , 132 That it consists of two resins represented respectively by the formulae ( analyses 4 , 7 , 8 , and 31 , 32 ) .
The soluble , or resin A. by C40 H31 04 an acid resin .
The insoluble , or resin B. by C40 H31 02 not an acid .
2 .
That even when considerable care is taken , a series of analyses may be obtained which do not indicate the true constitution of a resin ( see analyses 1 , 2 , 3 .
) .
3 .
That when exposed to the prolonged action of a temperature exceeding 3000 FAHR. , resin A. of mastic , among other changes , seems to be partly altered into a resin containing three , and into one containing five of oxygen , C40 being constant ( analyses 6 , and 11 .
) .
These resins are probably represented by A =C40 H32 03 , very soluble in alcohol .
B= C40 H30 05 , sparingly soluble in alcohol .
4 .
That it combines with bases forming four series of salts , which in the case of oxide of lead consist of ( see analyses 14 , 15 , 16 , 17 .
) , 1 .
Two equivalents of resin and one of oxide .
2 .
Three equivalents of resin and two of oxide .
3 .
One equivalent of resin and one of oxide .
4 .
One equivalent of resin and two of oxide.* 5 .
That in combining with bases , resin A. does not part with any of its oxygen , but that if any change take place in its constitution it is in the hydrogen being replaced by an equivalent proportion of a metal ( analyses 19 , 21 , 22 , 23 , 24 , 25 , and 30 .
) .
The salts of lead would on this view be represented by 1 .
C40 131 04 + C40 1H30 Pbl 05 .
3 .
C40 H30 Pb 05 .
2 .
C40o I-31 04 +2 ( C40 H30 Pb1 05 ) .
4 .
C40 29 Pb2 06 .
I regret to be obliged to leave this interesting part of the subject in an undetermined state , but it will require many often repeated analyses to determine whether this law be generally obeyed by the resins in their combinations with bases .
6 .
That resin A. by boiling in contact with ammonia and nitrate of silverl , or perhaps with nitrate of ammoniat , is changed into a resin , represented , when uncombined , by C40 H32 03 .
This resin forms a bisalt with oxide of silver , in which there is also an apparent replacement of hydrogen by silver* , the resin in this salt ( analyses 24 and 25 ) being represented by C40 H3 03 .
IL .
Resin of Dragon 's Blood .
Two varieties of dragon 's blood are common in this country ; one in long stalks or quills enclosed in a leaf , or reed , and presenting the appearance of having been softened by heat previous to being rolled into this form ; the other in lumps of considerable size , less compact , and mixed with a large quantity of vegetable and other foreign matter .
1 .
The purer variety in quills gave , on digestion in alcohol , and evaporation of the solution on the water bath , a resin almost black by reflected light , translucent , in thin fragments , and of a bright red by transmitted light , and in powder of a dark red colour .
In preparing these resins it is difficult to determine at what temperature the whole of the alcohol or ether is driven off , and when the frothing up is due to the decomposition or disengagement of volatile matter from the resin itself .
This is especially the case in regard to such as , like the present , melt.at a low temperature .
If the solution in alcohol or ether be evaporated at 1800 FAHR. till it flows smooth and ceases to change in consistency , it will be found still to froth up and give off vapours having a peculiar , at first agreeable , afterwards astringent ( ?
) odour , if the heat be raised to 212 ? .
That a change of composition ensues from a greater increase of temperature appears from the following analyses .
A. A portion of the solution in alcohol was evaporated and heated for a short time at 212 ?
FAHR. 11'3 grains gave C= 29'43 , and H= 6'084 grains .
B. A second portion was evaporated at 212 ?
, and afterwards raised for a few minutes to 220 ?
FAHR. 11-16 grains gave C= 29*04 , and H= 6'135 grains .
C. The same heated to 2800 FAHR. frothed up , emitting vapours having an astrin.gent alcoholic odour , accompanied with considerable pungency .
It was still entirely soluble in alcohol .
boiling in water and drying at 3000 FAHR. , 10'04 grains gave C= 28'89 , and H= 9.445 grains , or per cent. Carbon _ 79-56 Hydrogen = 10'45 100 .
Oxygen = 9'98J By comparing this result with analyses 4 , 7 , and 8 , it will be seen that the resin had undergone no change in composition , but was still C40 Hsi 04 .
12*42 grains gave C= 32'965 , and H= 6'94 grains .
These results are equivalent to At 212 ? .
At 220 ? .
At 280 ? .
Carbon = 72'015 71*887 73-435 IHydrogen 5'982 6'108 6'208 Oxygen = 22'003 22'005 20-357 100 100 100 Had the results contained in the first and second columns been obtained fromin the same specimen , we might have concluded that up to 220 ?
FAHR. no sensible decomposition takes place .
As however these results , though they approximate to the formula 40 H20o 09 , are yet not accurately represented by any formlula in which the carbon is expressed by C40 , I thought it necessary to analyse the resin prepared by evaporating a solution at a temperature never exceeding 180 ?
FAHR. 2 .
For this purpose I took the common dragon 's blood in lumps , and digested two separate portions in alcohol and ether , and filtered and evaporatedthe solutions in broad shallow dishes .
The resin thus obtained was kept for twelve hours in a stove , the temperature of which was generally considerably under 180 ?
FAHR. At this temperature the resin from the ethereal solution was to the last softer , and contained more air-bubbles than that from the alcohol .
Both were of a brilliant red colour , contracted and cracked in every direction on cooling , and in fragments were exceeding electrical .
A. Of that from alcohol 10-25 graiins gave C= 27*523 , and II = 5.95 grains .
B. Of that from ether 11'65 grains gave C= 31-177 , and -H = 6'987 grains .
These are equal to A. B. Carbon -= 74247 = 73'998 Hydrogen = 6'450 = 6'663 Oxygen = 19'303 = 19'339 100 100 These results agree very nearly with the formula C40 H2 8 , , which gives 40 Carbon = 3057'480 = 74*218 21 Hydrogen = 262'091 = 6-362 8 Oxygen = 800000 = 19'420 4119'571 100 3 .
he close accordance of these results with a formula containing eight of oxygen induced me to return to the reed dragon 's blood , with the view of ascertaining whether the two varieties were really unlike in constitution , or whether the differences obtained by analysis might not result from the mode in which the resin was extracted , or the greater or less quantity of the solvent ( alcohol or ether ) they were permitted to retain .
A portion of it therefore was digested in ether , and the solution evaporated .
A. Evaporated and kept for twelve hours at 150 ?
FAHR. , 12*31 grains gave C 32-606 , and H= 6'757 .
B. Kept for twelve hours at 190 ?
FAHR. , 1112 grains gave C= 29'563 , and -I = 6-195 .
C. Of another portion evaporated at 212 ?
, and kept at this temperature for six hours , 11'97 grains gave C= 31'685 , and H 6'44 .
These results are equivalent to A. B. C. Carbon = 73'240 73'512 = 73'193 Hydrogen = 6'099 = 6'190 = 5'978 Oxygen = 20'661 20'298 = 20'829 100 100 100 Bv this prolonged heating of the resin obtained from the pipe or reed dragon 's blood ( as it is called in commerce ) , by means of ether , it is made to approximate nearer in constitution to the resin from the lump dragon 's blood than that which was first analysed .
Still there is a deficiency of nearly one per cent. in the carbon , and a considerable deficiency also in the hydrogen , compared with what is required by the formula C40 HI21 O as above given , and which is indicated by the analysis of the lump resin .
What is the cause of the difference , then , and which of the series of analyses is to be considered as representing the true constitution of the pure resin ?
I place most confidence in the series ( 2 .
) , for these reasons : first , the lump resin is mixed with seeds and fragments of vegetable matter , and is therefore most probably the resin as it exudes from the tree : second , the results of the analysis of this variety give an exact fortnula analogous to those by which so many other resins are represented , and of which the constant C40 is a member ; and third , the reed dragon 's blood , frop its porosity , its freedom from foreign substances , and its varying colour ( from a bright red to a dirty brown ) , is evidently a manufactured article , the constitution of which therefore is not to be depended upon .
Since I have been led to this conclusion , I have learned that a third variety of lragon 's blood is brought to the market under the name of strained .
Now to be strained the natural resin must be made very fluid , and can hardly fail to be more or less decomposed by the temperature necessary to produce the complete fuision .
The reed variety is probably only the strained , made wihile soft into small rolls and wrapped up .
Conclusions.-The following therefore seem to be the conclusions to which the above experiments lead .
136 That the lump dragon 's blood is the natural and pure resin , the strained and reed varieties being manufactured articles , and more or less decomposed .
2 .
That this resin retains alcohol and ether , as most other resins do , with considerable obstinacy , but that these solvents may be entirely expelled by a long-continued ( ten or twelve hours ) exposure to a temperature not higher than 200 ?
FAHR. 3 .
That when thus perfectly dried it is represented experimentally by the formula C40 H21 O8 .
The two former of these results are of considerable practical importance in an inquiry into the constitution of the resins .
Several of those resins which are of the greatest value in a commercial point of view , are said to be subjected to processes of manufacture , by the native collectors , before they are brought into the market ; it is therefore of consequence to ascertain that the substance is procured in its unaltered state before it is subjected to analysis .
I shall have occasion , in a subsequent patt of this inquiry , to mention several resins , the alteration of which by manufacture or adulteration has caused me much loss of time , and , in some cases , prevented me from obtaining a formula on which much reliance is to be placed .
In regard again to the total expulsion of the alcohol or ether , so necessary as solvents of this class of substances , if we evaporate the resins in mass , and heat till all the alcohol is driven off , we may often produce decomposition before our purpose is accomplished .
It is therefore of great importance to have learned , that long exposure of a thin film of the resin to a low temperature will fully deprive it of those volatile liquids .
Durham , March 12 , 1839 .