without cavities , and with uniformity , -a uniformity to be rendered perfect by subsequent pressure .
In order , however , to guard effectually against cavities , the barrel may be weighed after filling it , and the actual weight of its contents being thus ascertained , may be compared with that weight of platina and water which it is known by estimate that the barrel ought to contain* .
A circular piece of soft paper first , and then of woollen cloth , being laid upon the surface , allow the water to pass , during partial compression by the force of the hand with a wooden plug .
A circular plate of copper is then placed upon the top , and thus sufficient consistency is given to the contents to allow of the barrel being laid horizontally in a forcible press .
The press which I have generally used for this purpose , ( Plate I. ) , consists of a flat iron bar A B , set edgeways , and screwed down by a hook E , near its middle , where it would otherwise be liable to bend , to a strong wooden bench C D. The bar is connected by a pivot at its extremity A , with the lever AF G. An iron rod F I-I , which turns at its two extremities upon the pivots F and I- , proceeds from the lever at F , and , as the lever descends , propells forward the carriage I , which slides along the bar .
A stopper or block being placed in the vacant space I k , the carriage communicates motion to the cradle k1 m , which is also made to slide along the bar , and carries the barrel N , which lies upon the cradle , striaight against the piston 0 , which rests by its end against P , a projection in the further extremity of the bar .
The weight , which in this machine , when the angle of the lever 's elevation is small , will keep the power , applied vertically at the extrenity of the leve r,.AG x FH in equilibrio = that power X AF [ AF+ FHI X cotan .
of the angle of the lever 's elevation ; which expression , in the case of the press actually used , becomes , Power X 5 .
cotan .
of the angle of the lever 's elevation .
This expres ' From the mean weight of the ingots obtained in previous operations , it is known that the barrel described in the text ought to contain 16 ounces troy of dry platina powder .
The weight of the contents of the barrel = 16 ounces X sp , grav .
of platina 1+ the weight of a cubic inch of water sp. grav .
of platina 20.25 X capacity of the barrel in cubic inches = 16 ounces X 22125 +.526 ounces X 7.05 = 18.9575 21.25 ounces troy .
Should the contents of the barrel weigh materially less than this estimated weight , there must be a want of uniformity in the disposition of the powder within the barrel .
4 ^.7/ u/ I , ,.M -D1 ) CCCX XIX./ 4I,./ a. ; 1 ~~ ~ ~~~E _____- ' : 11l _______________Y_____=i____l_____~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~ IIi ii I* ii I sion , at an elevation of 50 , becomes nearly 60 X power , and at an elevation of 1 ?
, becomes nearly 300 X power ; and when the lever becomes horizontal , the multiplier of the power becomes quasi infinite .
This explanation will be sufficient to show the mechanical advantage with which , by means of this press , the weight of the operator , acting on the end of the lever , will be made to bear against the area of the section of the barrel , a circle little more than an inch in diameter .
After compression , which is to be carried to the utmost limit possible , the stopper at the extremity being taken out , the cake of platina will easily be removed , owing to the conical form of the barrel ; and being now so hardc and firm that it may be handled without danger of breaking , it is to be placed upon a charcoal fire , and there heated to redness , in order to drive off moisture , burn off grease , and give to it a firmer degree of cohesion .
The cake is next to be heated in a wind-furnace ; and for this purpose is to be raised upon a ern an arthen stand about 2 inches above the grate of the furnace , the stand being strown over with a layer of clean quartzose sand , on which the cake is to be placed , standing upright on one of its ends .
It is then to be covered with an inverted cylindrical pot , of the most refractory crucible ware , resting at its open end upon the layer of sand ; and care is to be taken that the sides of the pot do not touch the cake .
To prevent the blistering of the platina by heat , which is the usual defect of this metal in its manufactured state , it is essential to expose the cake to the most intense heat that a wind-furnace can be made to receive , more intense than the platina can well be required to bear under any subsequent treatment ; so that all impurities may be totally driven off , which any lower temperature might otherwise render volatile .
The furnace is to be fed with Staffordshire coke , and the action of the fire is to be continued for about twenty minutes from the time of lighting it , a breathing heat being maintained during the last four or five minutes .
The cake is now to be removed from the furnace , and being placed upright upon an anvil , is to be struck , while hot , on the top , with a heavy hammer , so as at one heating effectually to close the metal .
If in this process of forging , the cylinder should become bent , it should on no account be hammered on the side , by which treatment it would be cracked irremediably ; but must be 5 straightened by blows upon the extremities , dexterously directed , so as to reduce to a straight line the parts which project .
The work of the operator is now so far complete , that the ingot of platina may be reduced , by the processes of heating and forging , like that of any other metal , to any form that may be required .
After forging , the ingot is to be cleaned from the ferruginous scales which its surface is apt to contract in the fire , by smearing over its surface with a moistened mixture of equal parts by measure of crystallized borax and common salt of tartar , which , when in fusion , is a ready solvent of such impurities * , and then exposing it , upon a platina tray , under an inverted pot , to the heat of a wind-furnace .
The ingot on being taken out of the furnace , is immediately to be plungedl into dilute sulphuric acid , which in the course of a few hours will entirely dissolve the flux adhering to the surface .
The ingot may then be flattened into leaf , drawn into wire , or submitted to any of the processes of which the most ductile metals are capable .
The perfection of the methods above described , for giving to platina complete malleability , will best be estimated by comparing the metal tliuLs obtained , in respect of its specific gravity , with platina which has undergone complete fusion ; and by comparing it , in respect of its tenacity , with other metals possessing that quality in the greatest perfection .
The specific gravity of platina , drawn into fine wire , from a button which had been completely fused by the late Dr. E. D. CLARKE with an oxy-hydrogen blowpipe , I found to be 21.16 .
The aggregate specific gravity of the cake of metallic mud , when first introduced into the barrel , exclusively of moisture , is about 4.3 ; when taken from the press , is about 10 .
That of the cake fully contracted , on being taken out of the wind-furnace before forging , is from 17 to 17.7 .
The mean specific gravity of the platina , after forging , is about 21.25 , although that of some rods , after being drawn , is 21.4 : but that of fine platina wire , determined by comparing the weight of a given length of it with the weight of an equal length of gold wire drawn through the same hole , I find to be 21.5 , which is the maximum specific gravity that we can well expect to be given to platina .
The mean tenacity , determinedby the weights required to break them , of two fine platina wires , the one of the other of i of an inch in diameter , reduced to the standard of a wire -foth of an inch in diaineter , I found to be 409 pounds ; and the mean tenacity of 11 wires , beginning with oo and ending with 24-0o of an inch , reduced to the former standard , I found to be 589 pounds ; the maximum of these 11 cases being 645 pounds , and the minimum 480 pounds .
The coarsest and the finest wire which I tried , present exceptions , since a wire of T-5-lou of an inch gave 290 pounds , and a wire of 3y.000 of an inch , 190 pounds .
If we take 590 pounds , as determined by the 11 consecutive trials , to be the measure of the tenacity of the platina prepared by the processes above described , and consider that the tenacity of gold wire , reduced to the same standard , is about 500 , and that of iron-wire , 600 , we shall have full reason to be satisfied with the processes , detailed in the present paper , by which Platina has been rendered malleable .
To this paper I beg to subjoin an account of some processes relating to two of the metals which are found in the ore of platina .
To obtain malleable Palladium , the residuum obtained from burning the prussiate of that metal is to be combined with sulphur , and each cake of the sulphlluret , after being fused , is to be finally purified by cupellation , in an open crucible , with borax and a little nitre .
The sulphuret is then to be roasted , at a low red heat , on a flat brick , and pressed , when reduced to a pasty consistence , into a square or oblong and perfectly flat cake .
It is again to be roasted very patiently , at a low red heat , until it becomes spongy on the surface .
During this process , sulphur flies off in the state of sulphurous acid , especially at those moments when the heat is allowed occasionally to subside .
The ingot is then to be cooled ; and when quite cold , is to be tapped with a light hammer , in order to condense and beat down the spongy excrescences on its surface .
The alternate roastings and tappings ( or gentle hammerings ) require the utmost 7 patience and perseverance , before the cake can be brought to bear hard blows : but it may , by these means , at length be made so flat and square , as to bear being passed through the flatting-mill , and so laminated to any required degree of thinness .
Thus prepared , it is always brittle , while hot ; possibly , from its still containing a small remnant of sulphur .
I have also fused some palladium per se , without using sulphur ; but I have always found it , when treated in this way , so hard and difficult to manage , that I greatly prefer the former process .
To obtain the oxide of Osmium in a pure , solid , and crystallized state , I grind together , and introduce , when ground , into a cold crucible , 3 parts by weight of the pulverulent ore of iridium , and 1 part of nitre .
The crucible is to be heated to a good red in an open fire , until the ingiredients are reduced to a pasty state ; when osmic fumes will be found to arise from it .
The soluble parts of the mixture are then to be dissolved in the smallest quantity of water necessary for the purpose , and the liquor , thus obtained , is to be mixed , in a retort , with so much sulphuric acid , diluted with its weight of water , as is equivalent to the potash contained in the nitre employed ; but no inconvenience will result from using an excess of sulphuric acid .
By distilling rapidly into a clean receiver , for so long a time as the osmic fumes continue to come over , the oxide will be collected in the form of a white crust on the sides of the receiver ; and there melting , it will run down in drops beneath the watery solution , forming a fluid flattened globule at the bottom .
When the receiver has become quite cold , the oxide will become solid and crystallize .
One such operation has yielded 30 grains of the crystallized oxide , besides a strong aqueous solution of it .
LECTURE.-On a method of rendering Platina malleable .
By WILLIAM HYDE WOLLASTON , M.D. F.R.S. SSc .
Read November 20 , 1828 .
AS , from long experience , I probably am better acquainted with the treatment of Platina , so as to render it perfectly malleable , than any other member of this Society , I will endeavour to describe , as briefly as is consistent with perspicuity , the processes which I put in practice for this purpose , during a series of years , without seeing any occasion to wish for further improvement .
The usual means of giving chemical purity to this metal , by solution in aqua regia and precipitation with sal ammoniac , are known to every chemist ; but I doubt whether sufficient care is usually taken to avoid dissolving the Iridium contained in the ore , by due dilution of the solvent .
In an account which I gave in the Philosophical Transactions for 1804 , of a new metal , Rhodium , contained in crude platina , I have mentioned this precaution , but omitted to state to what degree the acids should be diluted .
I now therefore recommend , that to every measure of the strongest muriatic acid employed , there be added an equal measure of water ; and moreover , that the nitric acid used be what is called " single aquafortis ; " as well for the sake of obtaining a purer result , as of economy in the purchase of nitric acid .
With regard to the proportions in which the acids are to be used , I may say , in round numbers , that muriatic acid , equivalent to 150 marble , together with nitric acid equivalent to 40 marble , will take 100 of crude platina ; but in order to avoid waste of acid , and also to render the solution purer , there should be in the menstruum a redundance of 20 per cent at least of the ore .
The acids should be allowed to digest three or four days , with a heat which ought gradually to be raised .
The solution , being then poured off , should be suffered to stand until a quantity of fine pulverulent ore of iridium , suspended in the liquid , has completely subsided ; and should then be mixed with 41 parts of sal ammoniac , dissolved in about 5 times their weight of water .
The first precipitate , which will thus be obtained , will weigh about 165 parts , and will yield about 66 parts of pure platina .
As the mother-liquor will still contain about 11 parts of platina , these , with some of the other metals yet held in solution , are to be recovered , by precipitation from the liquor with clean bars of iron , and the precipitate is to be redissolved in a proportionate quantity of aqua regia , similar in its composition to that above directed to be used : but in this case , before adding sal ammoniac , about 1 part by measure of strong muriatic acid should be mixed with 32 parts by neasure of the nitro-muriatic solution , to prevent any precipitation of palladium or lead along with the ammonio-muriate of platina .
The yellow precipitate must be well washed , in order to free it from the various impurities which are known to be contained in the complicated ore in question ; and must ultimately be well pressed , in order to remove the last remnant of the washings .
It is next to be heated , with the utmost caution , in a black-lead pot , with so low a heat as just to expel the whole of the sal ammoniac , and to occasion the particles of platina to cohere as little as possible ; for on this depends the ultimate ductility of the product .
lThe gray product of platina , when turned out of the crucible , if prepared with due caution , will be found lightly coherent , and must then be rubbed between the hands of the operator , in order to procure by the gentlest means , as much as can possibly be so obtained , of inmetallic powder , so fine as to pass through a fine lawn sieve .
The coarser parts are then to be ground in a wooden bowl with a wooden pestle , but on no account with any harder material , capable of burnishing the particles of platina* ; since every degree of burnishing will prevent the particles from cohering in the further stages of the process .
Since the whole will require to be well washed in clean water , the operator , in the later stages of grinding , will find his work much facilitated by the addition of water , in order to remove the finer portions , as soon as they are sufficiently reduced to be suspended in it .
Those who would view this subject scientifically should here consider , that as platina cannot be fused by the utmost heat of our furnaces , and consequently cannot be freed like other metals , from its impurities , during igneous fusion , by fluxes , nor be rendered homogeneous by liquefaction , the mechanical diffusion through water should here be made to answer , as far as may be , the purposes of mnelting ; in allowing earthy matters to come to the surface by their superior lightness , and in making the solvent powers of water effect , as far as possible , the purifying powers of borax and other fluxes in reminoving soluble oxides .
By repeated washing , shaking , and decanting , the finer parts of the gray powder of platina may be obtained as pure* as other metals are rendered by the various processes of ordinary metallurgy ; and if now poured over , and allowed to subside in a clean basin , a uniform mud or pulp will be obtained , ready for the further process of casting .
The mould which I have used for casting , is a brass barrel , 6a inches long , turned rather taper within , with a view to facilitate the extraction of the ingot to be formed , being 1.12 inches in diameter at top , and 1.23 inches at a quarter of an inch from the bottom , and plugged at its larger extremity with a stopper of steel , that enters the barrel to the depth of a quarter of an inch .
The inside of the mould being now well greased with a little lard , and the stopper being fitted tight into the barrel by surrounding it with blotting-paper , ( for the paper facilitates the extraction of the stopper , and allows the escape of water during compression , ) the barrel is to be set upright in a jutg of water , and is itself to be filled with that fluid .
It is next to be filled quite full with the mud of platina ; which , subsiding to the bottom of the water , is sure to fill the barrel become firmly welded together ; but if the surfaces have previously been burnished with any hard substance , the welding will be effected , if at all , with very great difficulty .
When the powder of platina has been over-heated in decomposing the ammonio-muriate , or has been burnished in the grinding , I have in vain endeavoured to give it a welding surface , by steeping it in a solution of sal-ammoniac in nitric acid .