VIII .
Experiments on Wootz .
By Mr. David Mushet .
Communicated by the Right Hon. Sir Joseph Banks , K. B. P. R. S. Read February 14 , 1805 .
THE following experiments were made at the request of Sir JOSEPH BANKS , on five cakes of wootz , with which he supplied me for that purpose .
As the cakes , which were numbered 1 , 2,3 , 4,5A , were not all of the same quality , it will be proper first to describe the differences observable in their external form and appearance .
No. i was a dense solid cake , without any flaw or fungous appearance upon the flat , or , what I suppose to be , the upper side .
The round or under surface was covered with small pits or hollows , two of -which were of considerable depth ; one through which the slit or cut had run , and another nearly as large towards the edge of the cake .
These depressions , the effects , as I suppose , of a species of crystallization in cooling , were continued round the edges , and even approached a little way upon the upper surface of the wootz .
The cake was a quarter of an inch thicker at one extremity of the diameter than at the other , from which I infer , that the pot or crucible , in which this cake had been made , had not occupied the furnace in a vertical position .
Its convexity , compared to that of the other fivewas second .
Upon breaking the thin fin of steel , which connects the haif cakes together , I found it to possess a , very small dense white grain .
This appearance never takes Y X place but with steel of the best quality , and is less frequent in very high steel , though the quality be otherwise good .
Upon examining the break with attention , I perceived several laminae and minute cells filled with rust , which in working are never expected to unite or shut together .
The grain otherwise was uniformly regular in point of colour and size , and possessed a favourable appearance of steel .
No. 2 .
This cake had two very different aspects ; one side was dense and regular , the other hollow , spongy , and protuberant .
The under surface was more uniformly honeycombed than No. 1 ; the convexity in the middle was greater , but towards the edges , particularly on one side , it became flatter .
The grain exposed by breaking was larger , bluer in colour , and more sparkling than No. i. In breaking , the fracture tore b-it slightly out , and displayed the same unconnected laminae with rusty surfaces , a , were observed in No. i. Beside these , two thin fins of malleable iron projected from the unsound side , and seemed incorporated with the mass of steel throughout .
Towards the centre of the break , and near to the excrescence common to all the cakes , groups of malleable grains were distinctly visible .
The same appearance , though in a slighter degree , manifested itself in various places throughout the break .
No. 3 .
The upper surface of this cake contained severaldeep pits , which seemed to result from the want of proper fluidity in fusion .
They differed materially from those described upon the convex sides of No. i and 2 , and were of that kind that would materially effect the steel in forging .
The under or convex side of this cake presented a few crystalline depressions , and those very small ; the convexity was greater than that of No. i and 2 , the fracture of the fin almost smooth , and only in one place exhibited a small degree of tenacity in the act of parting .
In the middle of the break , about half an inch of soft steel was evident ; and in different spots throughout numerous groups of malleable grailns , and thin laminae of soft blue tough iron made their appetarnoe .
No. 4 .
Was a thick dense cake possessed of the greatest convexity ; the depressions upon the under side were neither so large , nor so numerous as those in No. i and 2 , nor didthey approach the upper surface of the cake further than the acute edge .
This surface had the most evident marks of hammering to depress the feeder , or fungous part of the metal , which in the manufacturing seems the gate or orifice by which the metal descends in the act of gravitation .
The break of this cake , however favourable as to external appearance , was far from being solid .
Towards the feeder it seemed loose and crumbly , and much oxidated The grain divided itself into two distinct strata , one of a dense whitish colour , the other large and bluish , containing -a number of small specks of great brilliancy .
Several irregular lines of malleable -iron pervaded the mass in various places , which indicated a compound too heterogeneous for good steel .
5th cake .
This was materially different in appearance from any of the former .
It had received but little hammering , yet was smooth and free from depressions , or honey-comb on both surfaces .
The feeder , instead of being an excrescenoe , presented a deep concave beautifully crystallized .
In breaking , the fracture tore out considerably , but presented a very irregular quality of grain .
That towards the under surface was small and uniform , but towards the flat or upper surfaces it increased in size , and in the blueness of its -colour , till it passed into the state of malleable iron .
The break of this steel , though apparently soft , was the least homogeneous of the whole , and throughout it presented a very brilliant arrangement of crystal , which in other steel is always viewed with suspicion .
General Remark .
Uniformly the grain and density of the wootz are homogeneous , and free from malleable iron towards the under or round surface ; but always the reverse towards the feeder or upper side .
Remarks in Forging .
No. i. One-half of the cake was heated slowly by an annealing heat to a deep red , and put under a sharp broad-mouthed chisel with a small degree of taper .
It cut with difficulty , was reheated , and cracked a little towards one end of the slit or cut originally in the cake .
The heat in this trial was so moderate , that I was afraid that the crack had arisen from a want of tenacity , occasioned by the heat being too low .
The other half was heated a few shades higher , and sub .
jected to the same mode of cutting ; before the chisel had half way reached the bottom , the piece parted in two in the direction of them depression made by the cutting instrument .
The additional heat in this instance proved -an injury , while the cracking of the steel in both cases , particularly the former , was a certain proof of the abundance , or rather of the excess of the steely principle .
Thie fractures of both half cakes , now obtained for a second time , were materially different from that obtained by the simple division of the cake .
The grain was nearly uniform , distinctly marked , but of too gray a colour for serviceable steel .
Two of the quarters being drawn into neat bars under hand hammers at a low heat , one of them contained a number of cracks and fissures .
The fracture was gray , tore out a little in breaking , but was otherwise yolky ... and .
excessively dense .
A small , bar of penknife size was improved greatly in drawing .
down , and had only one crack in thirteen inches of length , ; The .
grain and fracture were both : highly improved by this addi- .
, tional labour ; the tenacity of the steel was .
greater , and it : stood firmly under the hammer at a bright red heat .
The other two quarters of this cake were squared a little , , and successively put under a tilt hammer , of two hundred weight , going at the rate of three hundred -blows per minute , and drawn into small penknife size .
One of the bars from an outside piece , always the most.-solid , -was:entirely free fromcracks , and had only one small scale running upon one side .
These bars exhibited a tougher break , than those drawn by hand ; the colour was whiter and the grain possessed a more regular and silky appearance .
Forging No. 2 .
" 'One half of this cake was heated to a scarlet shade , and put .
under the cutting chisel it was at first struck lightly , then reheated , and cut comparatively soft ; but a small crack had , over-run the progress of the chisel .
Its softness in cutting was attributed to an .
evident want of solidity .
The other half cake felt , harder ufider the hammer , but proved afterwards spongy throughout the mass .
In the act of cutting , a loose pulverised matter was disengaged from some of the cells , possessed of a shining appearance .
The fractures obtained in consequence of the division of the half cakes , presented a flattish crystallized appearance , more resembling very white -cast iron , than steel capable of being extended under the hammer .
One of the middle cuts was entirely cellular with crystallized interiors , and incapable of drawing ; the corresponding cut of the other hatf cake was drawn into a straight bar three quarters of an inch in breadth , and three-eighths thick , but was covered with cracks and flaws from end to end .
The colour of the break was one shade lighter than No. i , it tore less out , was equally yolky , and possessed on the whole an aspect very unfavourable for good steel .
The other two outside quarters were also drawn into shape , one under the tilt hammer , and the other by hand .
These were more solid in the fracture , possessed fewer surfacecracks , stood a higher degree of heat , tore out more , and exhibited a silky glossy grain , at least two shades lighter in the colour than the centre pieces .
Forg-ing 3d Cake .
One half of this cake , first subjected to be cut , was found softer than any of the preceding , and exhibited no symptom of cracking .
The other half was cut at three heats , but found loose and hollow in the extreme .
A considerable portion of the same brilliant powder , formerly noticed , was here again disengaged .
It was carefully taken up for examination , and found to be very fine ore of iron in a pulverescent state , very obedient to the magnet , and without any doubt an unmetallized portion of that from which wootz is made .
This curious circumstance led me to examine every pore and cell throughout the whole fragments .
On the upper surface of two of them I found small pits containing a portion of the ore , which had been slightly agglutinated in the fire , but still highly magnetic .
The upper surface of the present cake , close by the gate or feeder , contained a large pit filled with a stratum of semi-fused ore , surmounted by a mass of vitrified matter , which bore evident marks of containing calcareous earth .
Those who have devoted sufficient attention to the affinities of iron and earths for carbon , will be surprised to find that , on this particular subject , the rude fabricators of steel in Hindostan have got the start of ; our more polished countrymen in the manufacture of steel .
Two bars of wootz were formed from this cake , and these in point of quality inferior to any of those formerly produced .
The appearance of the metal was more varied , less homoge .
neous , and contained more distinct laminae with rusty surfaces , than either of the two former cakes .
It appeared highly probable , from the observations that oc .
curred in forging , and in the examination of the cake , that the original proportion of mixture was such as would have formed a quality of steel softer than No. 1 and , ; but as steel of such softness requires a greater heat to fuse it , than when more fully saturated with carbonaceous matter , it is probable that the furnace had not been sufficiently powerful to occasion complete fusion of the whole mass , and generate a steel homogeneous in , all its parts .
Forging h4t Cake .
Both halves of this cake cut , pleasantly ad with -a degree of tenacity and resistance , mixed at the same time with softness beyond what was experienced in any of the former cakes .
Two quarters of this cake were drawn under the tilt hammer , and one by hand .
The resulting bars were nearly perfect .
A slight scale was observable upon the bar , from that quarter which contained the figure .
The fracture was solid , though not homogeneous as to quality and colour , and it appeared pretty evident , that a considerable portion of one side through the whole bar was in the state of : malleable iron , and of corse not capable of being hardened .
It was a subject of considerable regret , that the cake the most perfect and the most tena- .
Cious of the whole , in the process of forging , should get an imperfection which rendered it useless for the perfect purposes of steel .
Forging 5th Cake .
The first half of this cake cut uncommonly soft for wootz , but by cracking before the chisel still exhibited a want of proper tenacity .
The next half cut equally soft , but with more tenacity .
Two quarters of this cake drew readily out under the tilt hammer , and a third was drawn by hand at a bright red , sometimes approaching to a faint white heat .
None of the bars thus obtained were uniformly free from cracks and scale , although the .
fracture exhibited a fair break of a light blue colour , and the grain was distinctly marked , and free from yolks .
General Remarks .
The formation of wootz appears to me to be in consequence of the fusion of a peculiar ore , perhaps calcareous , or rendered highly so by mixture of calcareous earth along with a portion of carbonaceous matter .
That this is performed in a clay or other vessel or crucible , is equally presumable , in which the separated metal is allowed to cool ; hence the crystallization that occupies the pits and cells found in and upon the under or rounded surface of the wootz cakes .
The want of homogeneity , and of real solidity in almost every cake of wootz , appears to me to be a direct consequence of the want of heat sufficiently powerful to effect a perfect reduction ; what strengthens this supposition much is ) that those cakes that are the hardest , I. e. that contain the greatest quantity of carbonaceous matter , and of course form the most fusible steel , are always the most solid and homogeneous .
` On the contrary , those cakes , into which the cutting chisel most easily finds its way , are in general cellular , replete with laminx , and abound in veins of malleable iron .
It is probable , had the native Hindostan the means of rendering his cast steel as fluid as water , it would have occurred to him to have run it into moulds , and by this means have acquired an article uniform in its quality , and convenient for those purposes to which it is applied .
The hammering , which is evident around the feeder and upon the upper surface in general , may thus be accounted for .
When the cake is taken from the pot or crucible , the feeder will most probably be slightly elevated , and the top of the cake partially covered with small masses of ore and steel iron , Z7 which the paucity of the heat had left either imperfectly separated or unfused .
These most probably , to make the product nor marketable are cut off at a second heating , and the whole surface hammered smooth .
I have observed the same facts and similar appearances in operations of a like nature , and can account satisfactorily for it as follows .
The first portions of metal , that are separated in experiments of this nature , contain the largest share of the whole carbon introduced into the mixture .
It follows of course , that an inferior degree of heat will maintain this portion of metal ina state of fluidity , but that a much higher temperature isrequisite to reduce the particles of metal , thus for a season robbed , of their carbon- , and bring them into contact with the portion first rendered fluid , to receive their proportion of the steely principle .
Where the heat is languid , the descent of the last portions of iron is sluggish , the mass below begins to lose its fluidity , while its disposition for giving out carbon is reduced by the gradual addition of more iron .
An accumulation takes place of metallic masses of various diameters , rising up for half an iinch or more into the glass that covers the metal ; these are neatly welded and inserted into each other , and diminish in diameter as they go up .
The length , or even the existence of this feeder or excrescence , depends upon the heat in general , and upon its temperature at different periods of the same process .
If there has been sufficient heat , the surface will be convex and uniformly crystalline ; but if the heat has .
been urged , after the feeder has been formed and an affinity established between it and the steelified mass below , it will only partially disappear in the latter , and the head or part of the upper end of the feeder will be found suspended in the glass that covers the steel .
The same or similar phenomena take place in separating crude iron from its ores , when highly carbonated , and difficult , from an excess of carbon , of being fused .
The division of the wootz cake by the manufacturers of Hindostan , I apprehend is merely to facilitate its subsequent application to the purposes of the artist ; it may serve at the same time as a test of the quality of the steel .
To ascertain , by direct experiment , whether vootz owed its hardness to an extra quantity of carbon , the following experiments were performed with various portions of wootz of common cast steel , and of white crude iron , premising that in operations with iron and its ores , I have always found the comparative measure of carbon best ascertained by the quantity of lead which was reduced from flint glass .
1st ( Cake .
Grains .
Fragments of wootz 65 Pounded flint glass three times the weight 195 This mixture was exposed to a heat of 1600 WEDGEWOOD , and the wootz fused into a well crystallized spherule of steel .
A thin crust of revived lead was found below the wootz , which weighed 9 grains , or I1 3092 the weight of the wootz .
2d Cake .
Fragments of wootz 8o Flint giass , same proportion as above 240 The fusion of the mixture in this experiment was productiveof a mass of lead weighing io grains , equal to 8th the weight of the wootz .
3d Cake .
Grains .
Fragments of wootz 75 Flint glass H225 The mass of lead precipitated beneath the steel in this experiment , amounted to 9 grains or the weight of the wootz employed .
4th Cake .
, Fragments of wootz 93 Flint glass 279 Lead obtained , precipitated from the glass by means of the carbon of the wOotz 14i grains , equal to 5 the weight of the wootz .
-th Cake .
Fragments of wo-otz a -Flint glass 207 The lead revived in this experiment amounted to 7 grains , which is equal to ?
'OJ the weight of the wootz .
6th .
Cast Steelformed with gth part its Weight of Carbon .
Fragments go Crystal glass A 270 Lead revived 82grains equal to ; the weight of the steel introduced .
7th .
Jhite cast Iron dropped while Fluid into Water .
Fragments _3 Crystalglass __ 09 The fusion of this precipitated 23j grains of lead which is equal to -2-L the , weight of the cast iron .
Recapitulation of these Experiments .
ist cake of wootz revived of lead,39 2d ditto c125 3d ditto -20 4th ditto,156 , th ditto _ Steel containing B of its weight of carbon _ , i Cast iron 228 It would appear to result from these experiments , that wootz contains a greater proportion of carbonaceous matter , than the common qualities of cast steel in this country , and that some particular cakes approach considerably to the nature of cast iron .
This circumstance , added to the imperfect fusion which generally occurs in the formation of wootz , appear to me to be quite sufficient to account for its refractory nature , and unhomogeneous texture .
Notwithstanding the many imperfections with which wootz is loaded , it certainly possesses the radical principles of good steel , and impresses us with a high opinion of the ore from which it is formed .
The possession of this ore for the fabrication of steel and bar iron , might to this country be an object of the highest importance .
At present it is a subject of regret , that such a source of wealth cannot be annexed to its capital and talent .
Were such an event practicable , then our East India Company might , in their own dominions , supply their stores with a valuable article , and at a much inferior price to any they send from this country .