XVI .
Directions for making the best Composition for the Metals of reflecting Telescopes ; together with a Description of the Process for grinding , polishing , and giving the great Speculum the true parabolic Curve .
By Mr. John Mudge ; communicated by Alexander Aubert , Esq. F. R. S. AS the method of casting , grinding , and polishing the specula of reflecting telescopes , by Mess .
MOLYNEUX and HADLEY , which is published in Dr. SMITH'S Optics , is what the workmen have generally followed , and is consequently well known to them ; I shall in the following account avoid a repetition of the general directions there given , and only remark upon such parts of that process which I think are essentially defective , and supply them by a method of my own , which , from long and repeated trials , I have found completely to answer the purpose .
After , therefore , referring to the above account for the manner of making the gages , patterns , the method of casting , as well as a great many other particulars , I will begin with The Read Feb. 27 .
March 6 .
and 13 , The best composition for the specula of reflecting telescopes .
The perfection of the metal of which the speculum should be made consists in its hardness , whiteness , and compactness ; for upon these properties the reflective powers and durability of the speculum depend .
And first of the hardness and whiteness of the metal .
There are various compositions recommended in SMITH'S Optics , all which have however their several defects .
Three parts copper and one part and one-fourth of tin will make , he says , a very hard white metal ; but it is liable to be porous .
This , however , is an imperfection which I shall presently show the method of preventing ; but the permanent fault of it , and which I have myself experienced , is , that it is not hard enough .
The speculum of a reflecting telescope ought to have the utmost possible hardness , compatible with its being operated upon by the tool .
It is to be observed , that ever so small a quantity of tin added to melted copper destroys its perfect malleability , and at the same time produces a metal whiter and harder than copper .
As the quantity of tin is increased , suppose to a fifth or fourth part , the metal becomes whiter , still harder , and consequently more friable .
If the quantity of tin be further increased to a third of the whole composition , it will then have its utmost whiteness ; but will be rendered at the same time so exceedingly hard and brittle , that the finest washed emery upon lead or brass will not cut it without breaking up its surface ; and the common blue stones used in grinding the speculum , will not touch it .
Mr. JACKSON ( some time since dead ) a mathematical-instrument-maker , and a most excellent workman , told me , that the tin was increased to the above proportion in his metals ; but that they were so exceedingly hard , that it cost him an infinite deal of pains , and a journey of two hundred miles , to find out a stone of sufficient hardness to cut it , and whose texture at the same time was fine enough not to injure its surface .
I have seen several of his finished metals ; they were indeed perfectly hard and white ; but the kind of stone with which he ground them he kept a secret .
After many experiments with various proportions of tin and copper , by gradually increasing the former , I at last found that fourteen ounces and an half of grain-tin to two pounds of good Swedish copper , made a beautiful white and very hard metal ; so hard indeed , that the stones would but barely cut it , and washed emery on brass or tin but just grind the surface without breaking it up ; whereas the proportion of tin being increased by the addition of only another half ounce , the former inconvenience venience immediately took place .
This therefore is the maximum in point of hardness .
Thus much of the two first considerations , the hardness and whiteness of the metal ; the next , and indeed the most essential , property is its compactness , or its being without pores .
This composition ( though complete in the former respects ) was , as well as Dr. SMITH 's , subject every now and then to be porous ; sometimes , indeed , I succeeded in casting a single metal , or perhaps two or three , without this imperfection ; at other times , and most frequently indeed , they were attended with this defect , without my being at all able to form a probable conjecture at the cause of my success or disappointment .
The pores were so very small that they were not discoverable when the metal had received a good face and figure upon the hones , nor till the last and highest polish had been given ; and then it frequently appeared as if dusted over with millions of microscopic pores , which were exceedingly prejudicial in two respects ; for first , they became in time a lodgment for a moisture which tarnished the surface ; and secondly , on polishing the speculum , the putty necessarily rounded off the edges of the pores , so as to spoil a great part of the metal , by the loss of as much light and sharpness in the image as there were defective points of reflection in the metal .
Besides the trouble of a great number of experiments , in order to get rid of this mischief , and to ascertain the cause to which it was owing , there was this additional inconvenience attending it , viz. that the fault was not discovered , as was observed before , till a great deal of trouble had been taken in grinding and even polishing the metal , the whole of which was rendered useless by the mortifying discovery of this defect .
I was extricated at last from this difficulty , and in some measure by accident .
Having one day made a great number of experiments , and having melted down all the good copper I had or could procure ; though puzzled and fatigued , yet not caring to give it up , I recollected that I had some metal which was reserved out of curiosity , and was a part of one the bells of St. Andrew 's which had been re-cast .
Expecting , however , very little from this gross and uncertain composition , I was nevertheless determined to see what could be made of it by enriching the composition with a little fresh tin .
Accordingly casting a metal with it , it turned out perfectly free from pores , and in every respect as fine a metal as ever I saw .
I could not at first conceive to what this success was owing ; but at last I hit upon the real cause of that defect , which had given me so much embarrassment and trouble during a course of near a hundred experiments , and in consequence thereof fell upon a method which ever after prevented it .
I had hitherto always melted the copper first , and when it was sufficiently fused , I used to add the proportional quantity of tin ; and as soon as the two were mixed , and the scoria taken off , the metal was poured into the moulds .
I began to consider that putty was calcined tin , and strongly suspected , that the excessive heat which the copper necessarily undergoes before fusion , was sufficient to reduce part of the tin to this state of calcination , which therefore might fly off from the composition in the sorm of putty , at the time the metal was poured into the flasks .
Upon this idea , after I had furnished myself with some more Swedish copper and grain-tin ( both which I had always before used ) I melted the copper , and having added the tin as usual to it , cast the whole into an ingot : this was , as I expected , porous .
I then melted it again , and as in this mixed state it did not acquire half the heat which was before necessary to melt the copper alone , so it was not sufficient to calcine the tin ; the speculum was then perfectly close , and free from this fault ; nor did I ever after , in a single instance , meet with the above mentioned imperfection .
All that is necessary , therefore , to be done to procure a metal which shall be white , as hard as it can be wrought , and perfectly compact , is to melt two pounds of Swedish copper , and when so melted , to add fourteen ounces and a half of grain-tin to it ; then , having taken off the scoria , to cast it into an ingot .
This metal must be a second time melted to cast the speculum ; but as it will fuse in this compound state with a small heat , and therefore will not calcine the tin into putty , it should be poured off as soon as it is melted , giving it no more heat than is absolutely necessary .
It is to be observed , however , that the same metal , by frequent melting , loses something of its hardness and whiteness : when this is the case , it becomes necessary to enrich the metal by the addition of a little tin , perhaps in the proportion of half an ounce to a pound .
And indeed when the metal is first made , if instead of adding the fourteen ounces and a half of tin to the two pounds of melted copper , about one ounce of the tin were to be reserved and added to it in the succeeding melting , before it is cast off into the moulds , the composition would be the more beautiful , and the grain of it much finer : this I know by experience to be the case .
The best method for giving the melted metal a good surface is this : the moment before it is poured off , throw into the crucible a spoonful of charcoal-dust ; imme2 diately diately after which the metal must be stirred with a wooden spatula , and poured into the moulds .
I wish I may not be considered as tedious in the above detail ; but as this business caused me a great deal of trouble , I was willing to give some account of the means by which I was freed from this difficulty ever after .
Perhaps , indeed , the whole of this process may be unnecessary , as many years since , I communicated this composition , and I believe at the same time the method of preventing the pores , to the late Mr. PETER COLLISON , a member of the Royal Society ; and likewise two or three years since , at the desire of my brother , to Mr. MICHELL .
Although it be possible , therefore , that this method is generally known , yet , as I have frequently of late seen specula with this defect , and observed metals of some of Mr. SHORT 's telescopes which are not quite so perfect as could be wished ( though they are all exquisitely figured ) I was willing by this publication wholly to remove any future embarrassment of this sort , and to furnish workmen with an excellent composition for their metals .
And would the Royal Society be pleased to honour the process with a place in their records , I know of no other method so proper to give this , as well as the following information , a general notoriety .
The metal being cast , there will be no occasion for the complicated apparatus directed by Dr. SMITH , for grinding and polishing it .
Four tools are all that are necessary , viz. the rough grinder to work off the rough face of the metal ; a brass convex grinder , on which the metal is to receive its spherical figure ; a bed of hones which is to perfect that figure , and to give the metal a fine smooth face ; and a concave tool or bruiser , with which both the brass grinder , and the hones are to be formed .
A polisher may be considered as an additional tool ; but as the brass grinder is used for this purpose , and its pitchy surface is expeditiously , and without difficulty formed by the bruiser , the apparatus is therefore not enlarged .
Of rough grinding the speculum .
The tool by which the rough surface of the metal is rendered smooth and fit for the hones , is best made of lead , stiffened with about a fifth or sixth part of tin .
This tool should be at least a third more in diameter than the metal which is to be ground ; and for one of any size , not less than an inch thick .
It may be cemented upon a block of wood , in order to raise it higher from the bench .
This leaden tool being cast , it must be fixed in the lathe , and turned as true as it is possible , by the gage , to the figure of the intended speculum , making a hole or pit in the middle , as a lodgment for the emery , of about an inch diameter for a metal of four inches : when this is done , deep grooves must be cut across its surface with a graver , in the manner represented in fig. 1 .
These grooves will serve to lodge the emery , and by their means the tool will cut a great deal faster .
There is no occasion to fear any alteration in the convexity of this tool by working the metal upon it , for the emery will bed itself in the lead , and so far arm the surface of it , that it will preserve its figure and cut the metal very fast .
Any kind of low handle , fixed on the back of the metal with soft cement , will be sufficient ; but it should cover two-thirds of its back to prevent its bending .
This way of working will cut the metal faster , and with more truth , than the method described by Dr. SMITH ; for should the surface and rough parts be attempted to be ground off by a common grind-stone by hand , though you did it as near the gage as possible , yet the metal would be so much out of truth when applied to the succeeding tool , that no time would be saved by it .
I used to employ a common labourer for this purpose , who soon acquired such a dexterity at working upon this tool , that in two hours time he would give a metal of four inches diameter so good a face and figure as even to fit it for the hones .
When all the sand-holes and irregularities on the face of the metal are ground off , and the whole surface is smooth and regularly figured , the speculum is then ready for the brass grinder , and must be laid aside for the present .
The manner of forming the brass-grinding tool .
The following is the method I have always pursued .
Procure a round stout piece of Hamburgh brass , at most a sixth part larger than the metal to be polished ; and let it be well hammered into a degree of convexity ( by the assistance of the gage ) suitable to the intended speculum .
Having done this , scrape and clean the concave side so thoroughly that it may be well tinned all over ; then cast upon it , after it has been pressed a proper depth into the sand , the former composition of tin and lead , in such quantity , that it may ( for a speculum of four inches diameter ) be at least an inch and an half thick , and with a base considerably broader than the top , in order that it may stand firmly upon the bench in the manner hereafter to be described .
This being done , it must be fixed and turned in the lathe with great care , and of such a convexity as exactly to suit the concave gage , which we suppose already made .
It will be necessary to be more careful in forming this than the former tool , and especially that no rings be left from the turning ; nor will the succeeding hone tool require so much exactness , as any defects in turning , will , by a method hereafter mentioned , be easily remedied ; but any inequality or want of truth in the brass tool will occasion a great deal of trouble before it can be ground out by the emery .
This tool must have a hole ( somewhat less than that in the metal to be worked upon it ) in the middle , quite through to the bottom .
When this tool is finished off in the lathe , its diameter should be one-eighth wider than the metal .
How to form the bed of hones , or the third tool .
Having chosen the kind of hones , and the best too , of the sort recommended in SMITH 's Optics ; they should be cemented in small pieces ( in a kind of pavement agreeably to his directions ) upon a thick round piece of marble , or metal made of lead and tin like the former composition ( which is what I have always used ) in such a manner , that the lines between the stones may run straight from one side to the other ; so that , placing the teeth of a fine saw in each of these divisions , they may be cleared from one end to the other of the cement which rises between the stones .
This bed of hones should be at least a fourth part larger than the metal which is to be ground upon it .
The surface of the metal upon which the hone pavement is to be cemented may or may not , as you please , be turned of a convexity suitable to the gage , though I have never taken that trouble .
As soon as the hones are cemented down , and the joints cleared by the saw , this tool must be fixed in the lathe , and turned as exactly true to the gage as possible ; which done , it must be laid aside for the present .
The next tool to be made is the bruiser .
The manner of forming the bruiser , the fourth and last tool .
This tool should be likewise made of thick stout brass like the former , perfectly sound , about a quarter of an inch thick , and hammered as near to the gage as possible .
It should be then scraped , cleaned , and tinned on the convex side , as the former tool was on the concave , and the same thickness of lead and tin cast upon it .
The general shape of this should differ from the former ; for as that increased in diameter at the bottom for the sake of standing firmly , so this should be only as broad at bottom as at top , as it is to be used occasionally in both those positions .
When this tool is fixed in the lathe , and turned off concave to the convex gage with great truth likewise , its diameter ought to be the middle size between the hones and the polisher .
Having with the lathe roughly formed the convex brass grinder , the bed of hones , and the concave bruisers , the convex and concave brass tools and the metal must be wrought alternately and reciprocally upon each other with fine emery and water , so as to keep them as nearly to the same figure as possible , in order to which some washed emery must be procured .
This is best done by putting it into a phial , which must be half filled with water and well shaken up , so that , as it subsides , the coarsest may fall to the bottom first , and the finest remain at the top : and whenever fresh emery is laid on the tools , the best method ( which we should also observe with the putty in polishing ) will be , to shake gently the bottle , and pour out a small quantity of the turbid mixture .
Of grinding the speculum , the brass tool , and the bruiser , together .
All the tools being ready , upon a firm post in the middle of a room , you are to begin to grind the brass convex tool with the bruiser upon it , working the latter crossways , with strokes sometimes across its diameter , at others a little to the right and left , and always so short that the bruisers may not pass above half an inch within the surface of the brass tool either way , shifting the bruiser round its axis every half dozen strokes or thereabout .
You must likewise , every now and then , shift your own position , by walking round , and working at different sides of the brass tool ; at times the strokes should be carried round and round , but not much over the tool : in short , they must be directed in such a way , and the whole grinding conducted in such a manner and with such equability , that every part of both tools may wear equally .
This habit of grinding , as well as the future one of polishing , will be soon acquired .
When you have wrought in this manner about a quarter of an hour with the bruiser upon the tool , it will be then necessary to change them , and , placing the bruiser upon its bottom , to work the convex tool upon that in the same manner .
When by working in this equable manner , alternately with the bruiser and tool , and occasionally adding fresh emery , you have nearly got out all the vestiges of the turning tool , and brought them both nearly to a figure , it will be then time to give the same form to the metal .
This must be done by now and then grinding it upon the brass tool with the same kind of emery , taking care however , by working the two former tools frequently together , to keep all three exactly in the same curve .
The best kind of handle for the metal is made of lead , a little more than double its thickness , and somewhat less in diameter , of about three pounds weight , with a hole in the middle ( for reasons to be shown hereafter ) a little larger than that in the metal : this handle should be cemented on with pitch .
The upper edge of this weight must be rounded off , that the fingers may not be hurt ; and a groove , about the bigness of the little finger , be turned round just below it , for the more conveniently holding and taking the metal off the tools .
The manner of figuring the metal upon the hones .
When the bruiser , brass tool , and metal , are all brought to the same figure , and have all a true good surface , the next part of the process is to give a correct spherical figure and a fine face to the metal , upon the hones .
It will be necessary to premise , however , that the hones should be placed in a vessel of water , with which they should be quite covered for at least an hour before they are used , otherwise they will be perpetually altering their figure when the metal comes to be ground upon them .
The same precaution is also necessary , if you are called off from the work while you are grinding the metal , for if they be suffered to grow dry , the same inconvenience will arise .
In order to give a proper figure to the hones , and exactly suitable to that of the brass tool , bruiser , and metal , when the hones are fixed down to the block , some common flour emery ( unwashed ) with a good deal of water must be put upon them , and the bruiser being placed upon the hones and rubbed thereon with a few strokes and a light hand , the inequalities of the stone will be quickly worn off ; but as a great deal of mud will be suddenly generated , it must be washed off every quarter of a minute with a great deal of water .
By a repetition of this , two or three times , the hones ( being of a very soft and friable substance ) will be cut down to the figure , without wearing or altering the bruiser at all .
Though this business may be quickly done , and can be continued but for a few strokes at a time , I need not say that it is necessary that those strokes be carried in the same direction , and with the same care , which was observed in grinding the former tools together .
As soon as the hones have received the general figure of the bruiser , and all the turning strokes are worn out from them , the emery must be carefully washed off ; in order to which , it will be necessary to clear it from the joints with a brush under a stream of water .
The bruiser and metal must be likewise cleared in the same manner , and with equal care , from any lurking particles of emery .
The hones being fixed down to the block , you now begin to work the bruiser upon them with very cautious , regular , short strokes , forward and backward , to the right and left , turning the axis of the bruiser in the hand while you move round the hones , by shifting your position , and walking round the block .
Indeed the whole now depends upon a knack in working , which should be conducted nearly in the following manner .
Having placed the bruiser on the centre of the hones , slide it in an equable manner forward and backward , with a stroke or two directly across the diameter , a little on one side , and so on the other ; then shifting your position an eighth part round the block , and having turned the bruiser in your hand about as much , give it a stroke or two round and round , but not far over the edges of the hones , and then repeat the cross strokes as before : those round strokes ( which ought not to be above two or three at most ) are given every time you shift your own position and that of the metals , previous to the cross ones , in order to take out any stripes either in the hones or bruiser , which may be supposed to be occasioned , by the straight cross strokes .
During the time of working , no mud must be suffered to collect upon the hones , so as to destroy the perfect contact between the two tools ; and therefore they must every now and then be washed clean by throwing some water upon them .
When by working in this manner all the emery strokes are ground off from the bruiser , and it has acquired a good figure and clean surface , you may then begin with the metal upon the hones , in the same cautious manner , washing off the mud as fast as it collects , though that will be much less now than when the bruiser was ground upon them .
Every now and then , however , the bruiser must be rubbed gently and lightly upon the hones , which will as it were , by sharpening them and preventing too great smoothness , occasion them to cut the metal much faster .
When , after having some time cautiously wrought in the manner before described , the hone-pavement has uniformly taken out all the emery strokes , and given a fine face and true figure to the metal , which will be pretty well known by the great equality there is in the feel while you are working , and by which an experienced workman will form a pretty certain judgment ; having proceeded thus far , I say , you may then try your metal , and judge of its figure by this more certain manner .
Wash the hone pavement quite clean ; then put the metal upon the center of it , and give two or three light strokes round and round only , not carrying , however , the edges of the metal much over the hones ; this will take out the order of straight strokes : then having again washed the hones , and placed the speculum upon their center , with gentle pressure , slide it towards you till its edge be brought a little over that of the hones , then carry it quite across the diameter as far the other side , and having given the metal a light stroke or two in this direction , take it off the tool .
The metal being wiped quite dry , place it upon a table at a little distance from a window ; stand yourself as near the window , at some distance from the metal , and looking obliquely on its surface , turn it round its axis , and you will see at every half turn the grain given by the last cross strokes flash upon your eye at once over the whole face of the metal .
This is as certain a proof of a true spherical figure as the operose and difficult method described in Dr. SMITH 's Optics ; for as there is nothing soft or elastic , either in the metal or in the hones , this glare is a certain proof of a perfect contact in every part of the two surfaces ; which there could not be if the spheres were not both perfect and precisely the same .
Indeed there is one accidental circumstance which necessarily affords its aid in this and every business of the like sort ; and that is , that a concave and convex surface ground together , though ever so irregular at first , will ( if the working be uniform and proper , consisting , especially at last , of cross strokes in every possible direction across the diameter ) be formed into portions of true and equal spheres ; had it not been for this lucky necessity , it would have been impossible to have produced that correctness which is essential in the speculum of a good reflecting telescope by any mechanic contrivance whatever .
For when it is considered , that the errors in reflection are four times as great as in refraction , and that the least defect in figure is magnified by the powers of the instrument , any thing short of perfection in the figure~ of the speculum would be evidently perceived by a want of distinctness in the performance .
I must not , however , quit this article without observing , that I all along suppose , both in forming the tools and at last figuring the metal ( and indeed the same must be observed in the future process of polishing ) that no kind of pressure is used that may endanger the bending or irregularly grinding them ; they should therefore be held with a light hand~ and loosely between the fingers , and the motion given should be in a horizontal direction , with no more pressure than their own dead weight .
Having now finished the metal on the hones , and rendered it both in point of figure and surface fit for the last and most essential process , viz. that of polishing , I will describe it in the best manner I can ; though many little circumstances which will be unavoidably omitted ( and which at the same time are frequently essential to the success of a mechanic process ) can only be supplied by actual experience .
The polishing the speculum is the most difficult and essential part of the whole process ; for every experienced workman knows , to his vexation , that the most trifling error here will be sufficient to spoil the figure of his metal , and render all his preceding caution useless .
I have , however , discovered a method which I shall explain , not only of giving the metal a parabolic figure , but also of recovering it when it happens to be injured ; both to be effected in the act of polishing , and the former as certainly as the spherical figure is given upon the hones .
Indeed , if we consider rightly , polishing will be perceived to be but a kind of grinding with a finer order of strokes , and with a powder infinitely finer than was before used in what is commonly called the grinding .
But before I describe this method , which was the result of many years experience , I will take the liberty of making some few strictures on that of Mess .
HADLEY and MOLYNEUX , which is followed by the generality of workmen .
First , then , the tool itself used by them for polishing the metal , is formed with infinite difficulty .
The first described polisher is directed to be made by covering the tool with sarcenet , which is to be saturated with a solution of pitch in spirit of wine , by successive applications of it with a brush , till it is covered , and by the evaporation of the spirit of wine filled with this extract of pitch ; the surface is then to be worked down and finished with the bruiser .
This is all very easy in imagination ; but whoever has used this method ( which I have myself unsuccessfully several times ) must have found it attended with infinite labour , and at last the business done in a very unsatisfactory manner ; for the pitch by this process will be deprived of an essential part of its composition .
The spirit of wine dissolves none but the resinous parts of its substance , which is hard and untractable ; and if you use soap or spirit of wine to soften or dissolve it , it will equally affect the whole surface , the lower as well as higher parts of it .
And suppose that with infinite labour with the bruiser , it is at last reduced to a fine uniform surface , it is nevertheless too hard ever to give a good polish with that lustre which is always seen in Mr. SHORT 's , and indeed all other good metals .
Nor will it give a good spherical figure ; for a perfect sphere is formed , as I observed before , by that intimate accommodation dation arising from the wear and yielding of both tool and metal ; whereas in this method , there is such a stubbornness in the polisher , that the figure of the metal , good or bad , must depend upon the truth of the former , which is very seldom perfect .
If the polisher be made in the second manner proposed , by straining the pitch through an outer covering , which is afterwards to be stripped off , the superficies of pitch and sarcenet is so very thin , that the putty , working into them , forms a surface hard and untractable , so that it is impossible to give the speculum a fine polish .
Accordingly all those metals which are wrought that way have an order of scratches instead of polish , discovering itself by a greyish visible surface .
Besides , supposing this tool perfectly finished , and answering its purpose ever so well , it is impossible it can produce in the speculum any other than a spherical figure ; and indeed nothing else is expected from this method , as very evidently appears by the experiment recommended to ascertain the truth of the figure .
You are directed to place a small luminous object in the center of the sphere of which the metal is a segment , and then having adjusted an eye-glass at the distance of its own focal length from the object , and so situated that the image of the object formed by the speculum may be visible to the eye , you are to judge of the perfect figure of the metal by the sharpness and distinctness with which the image appears .
From hence it is very evident , that as the object and image are both distant from the metal by exactly its radius , nothing but a true spherical figure of the speculum can produce a sharp distinct image ; and that the image could not be distinct if the figure of the speculum were parabolic .
Consequently , if the same speculum used in a telescope were to receive parallel rays , there would necessarily be a considerable aberration produced , and a consequent imperfection in the image .
Accordingly , there never was a good telescope made in this manner ; for if the number of degrees , or the portion of the sphere of which the great metal is a part , were as considerable as it ought to be , or as great as Mr. SHORT allowed in his metal , the instrument would bear but a very low charge , unless a great part of the circumference of the metal were cut off by an aperture , and the ill effects of the aberration by that means in some measure prevented .
If ever a finished metal turned out without this defect , and has been found perfectly sharp and distinct , it must have been owing to an accidental parabolic tendency , no ways the natural result of the process , and therefore quite unexpected , and most probably unknown , to the workman .
Without enlarging , therefore , on the difficulty of the above process , and the impossibility of giving the speculum the correctness and the kind of figure essentially necessary to a good telescope , I will describe ( by way of introduction to the succeeding directions ) the steps by which I was led to a certain and easy method of giving a proper and correct parabolic figure to the metal , even though it came off imperfect from the hones , and an exquisite polish at the same time .
Having made many efforts in the former method , which by no means pleased me for the reasons above-mentioned ; and having observed , from some of Mr. SHORT 's telescopes which fell into my hands , that the high lustre of the polish could never have been produced in the manner above described , but by some softer and more tender substance ; and at the same time recollecting , that Sir ISAAC NEWTON had given an account in his Optics of his having finished some metals , and considerably mended the object glass of a refractor , by working both upon a tool whose surface had been covered with common pitch about the thickness of a groat ; reflecting , I say , upon these matters ( coarse and uncertain as this method appeared at first sight ) I was determined to try whether I could not get rid of my embarrassment , by a mode of operation somewhat similar .
Accordingly , shortening Dr. SMITH 's process , I made a set of tools in the manner before described , except that I was obliged to make some subsequent alteration in the polisher which I shall presently describe .
Having given a good spherical figure to the brass tool and the bruiser , and likewise to the metal upon the hones , and made the brass convex tool so hot as just not to hurt the finger , I tied a lump of common pitch ( which should be neither too hard nor too soft ) in a rag , and holding it in a pair of tongs over a still fire where there was no rising dust , till it was ready to strain through the linen , I caused it to drop upon the several parts of the convex tool , till I supposed it would cover the whole surface about double the thickness of a shilling ; then spreading the pitch as equally as I could , I suffered the polisher ( by which name I shall for the future call this tool ) to grow quite cold .
I then warmed the bruiser so hot as almost to burn my fingers , and having fixed it to the bench with its face upwards , I suddenly placed the polisher upon it , and quickly slid it off ; by this means rendering the surface of the pitch more equal .
The pitch is then to be wiped off from the bruiser with a little tow ; and by touching the surface with a tallow candle , and wiping it a second time , it will be then perfectly clean and fit for a second process of the same sort , which must again be performed as quickly as possible ; and this is ordinarily sufficient to give a general figure to the surface of the pitch .
The bruiser and polisher are then suffered to grow perfectly cold , when the pitch , considering what has been taken off , will be about the thickness of a shilling .
It is however here necessary to observe , that the pitch should be neither very hard and resinous , nor too soft ; if the former , it will be so untractable as not to work kindly ; and if too soft , it will in working alter its figure faster than the metal , and too readily fit itself to the irregularity of its figure , if it have any .
When both tools were perfectly cold , I gave the polisher a gentle warmth , and then fixed the bruiser to the block with its face upwards ; and ( having with a large camel's-hair brush spread over the face of the polisher a little water and soap , to prevent sticking ) with short , straight , and round strokes I worked it upon the bruiser , every now and then adding a little more water and soap , till the pitch upon the polisher had a fine surface , and the true form of the bruiser ; and this I continued to do till they both grew perfectly cold together : in this manner the polisher was perfectly formed in about a quarter of an hour .
But here a difficulty arose : when I begun to polish the metal , I found that the edge of the hole in the metal collected the pitch towards the middle of the polisher ; and though in this method of working I could give an exquisite polish , as the putty lodged itself in the pitch exceedingly well , yet the figure of the metal was injured in the middle , nor did indeed the work go on with that equability which is the inseparable attendant on a good figure .
In order to obviate this difficulty , I cast some metals with a continued face , the holes not going quite through , within perhaps the thickness of a six-pence .
I finished two or three metals of this sort , and the work promised and went on very well ; but when I came to open the holes , which I did with the utmost caution , I found the metals short of perfection ; which I attributed to an alteration of the figure from the removal of even that small portion of metal after the speculum had been finished .
This I do suppose was in some measure the reason why I spoiled a very distinct and perfect two-foot metal , which bore a charge of two hundred times , only by opening the sharp part of the edge of the hole , because I thought it bounded the field : so essentially necessary is an exquisite correctness of figure in the speculum of a perfect reflector .
This experiment not succeeding , instead of casting the metal without a hole , I made one quite through the middle of the polisher , a little less than that in the speculum .
This perfectly answered the purpose ; no more inconvenience arose from the gathering of the pitch ( for it had now no greater tendency to collect at the center than the sides ) and I finished several metals successively , excellent both in point of figure and polish ; one of those of two inches diameter and 7,5 focal length , bore a charge of sixty times and upwards , which when mounted in a telescope I gave to my brother .
This telescope underwent Mr. SHORT 's examination , who was pleased to remark only , that he thought he had made one more distinct .
I must observe , that in this method of working the polishing goes on in an agreeable , uniform , and smooth manner ; and that the small degree of yielding in the pitch ( which is actually not more than the wearing of the metal ) produces that mutual accommodation of surfaces so necessary to a true figure .
In the beginning of the polish , and indeed for some time during the progress of it ( always remembering now and then to move the metal round its axis ) I worked round and round , not far from and always equally distant from the center , except that every time , previous to the shifting the metal on its axis , I used a cross stroke or two ; and when the polish was nearly completed , I mostly used cross strokes , giving a round stroke or two likewise every time I turned the metal on its axis .
I observed in this method of working , that the metal always polished fastest in the middle ; insomuch , that half or two-thirds of it would be completely polished when the circumference of it was scarcely touched by the tool .
Observing this in some of the first metals , and not considering that this way of polishing was in fact a species of grinding , and as perfect as that upon the hones , I went on reluctantly with the work , almost despairing of being able to produce a good figure .
However , I always found myself agreeably deceived ; for when the polish was extended to the edge , or within the tenth of an inch of it , I almost constantly found the figure good , and the performance of the metal very distinct .
But this same circumstance of apparent defect in the metals , was in fact that to which their perfection was owing ; for they all , contrary to my expectation , turned out parabolic .
However I did not for a great while know any certain way of giving that degree of parabolic tendency which was just necessary , and which will be described hereafter .
It was a long time before I got rid of my prejudice against this apparent imperfection in the process , or could reconcile myself to the irregular manner in which the polish proceeded ; for I looked upon it as a certain source of error , and notwithstanding I saw it eventually succeed , yet whenever I chanced to find that a metal , when first applied to the polisher , took the polish equally all over , and consequently the whole business did not take up above ten minutes ; under those circumstances , I say , I always used to please myself with the expectation of a correct figure , at least as much so as the metal had received from the hones , where the surface was but just and equally taken off by the putty ; but in this I constantly found myself deceived , and the metal turned out good for nothing .
In short , at this time , though I speculatively knew that a parabolic figure was necessary to a perfect image , I yet considered it as of little practical consequence .
From the foregoing experiments , and a number of succeeding trials , I at length discovered a certain way of giving a correct parabolic figure , and an exquisite polish at the same time .
This , which I have strong reasons to believe was Mr. SHORT 's method , I will now describe in as few words as I can .
How to polish the speculum .
It is first necessary to observe , that , in order to avoid the detrimental intrusions of any particles of emery , it would not be right to polish in the same room where the metal and tools were ground , nor in the same cloaths which were worn in the former process ; at least it would be necessary to keep the bench quite wet , to prevent any dust from rising .
Having then made the polisher by coating the brass convex tool equally with pitch , which we suppose smoothed and finished with the brass tool in the manner before described , and which is a very easy process , the whole operation is begun and finished in the following manner .
The leaden weight or handle upon the back of the metal should be divided into eight parts , by so many deep strokes of a graver upon the upper surface of the lead , marking each stroke with the numbers 1 , 2 , 3 , 4 , and so on , that the turns of the metal in the hand may be known to be uniform and regular .
To prevent any mischief from coarse particles of putty , I always wash it immediately before using .
In order to this , put about half an ounce of putty into an ounce phial , and fill it two-thirds with water ; then having shaken the whole , let the putty subside , and stop the bottle with a cork .
In a tea-cup with a little water , there should be a fullsized camel's-hair brush , and a piece of dry clean soap in a galley-pot : a soft piece of spunge will also be necessary .
These , as well as the metal bruiser and polisher , should be constantly covered from dust .
The polisher being fixed down , and the camel's-hair brush , being first wetted and rubbed a little over the soap , let every part of the tool be brushed over therewith ; then work the bruiser with short , straight , and round strokes , lightly upon the tool , and continue to do so , now and then turning it , till the polisher have a good face , and be fit for the metal .
Then having shaken up the putty in the phial , and touched the polisher in five or six places with the cork wetted with that and the water , place the bruiser upon the tool , and give a few strokes upon the putty to rub down any gritty particles ; after which , having removed it , work the metal lightly upon the polisher round and round , carrying the edges of the speculum , however , not quite half an inch over the edge of the tool , and now and then with a cross stroke .
The first putty , and indeed all the succeeding applications of it , should be wrought with a considerable while ; for if time be not given for the putty to bed itself in the pitch , and any quantity of it lie loose upon the polisher , it will accumulate into knobs , which will injure the figure of the metal : and therefore as often as ever such knobs arise , they must be carefully scraped off with the point of a penknife , and the loose stuff taken away with the brush .
After the putty is well wrought into the pitch , some more may be added in the same manner , but never much at a time , and always remembering to work upon it first with the bruiser , for fear any gritty particles may find their way upon the polisher .
If the bruiser be apt to stick , and do not slide smoothly upon the pitch , the surface of either tool may be occasionally brushed over with the soap and water , but it must be remembered that the wet brush must be but lightly rubbed upon the soap .
In the beginning of this process little effect is produced , and the metal does not seem to polish fast , in some measure owing to its taking the polish in the middle , and perhaps because neither that nor the bruiser move evenly upon the polisher : but a little perseverance will bring the whole into a good temper of working ; and , when the pitch is well defended by the coating of the putty , the process will advance apace , and the former acquiring possibly some little warmth , the metal moves more agreeably over it , with an uniform and regular friction .
All this while the metal must have no more pressure than that which it derives from its own weight and that of the handle ; and the polisher must never be suffered to grow dry , but , as often as it has any tendency to do so , the edges of it must be moistened with the hair-pencil ; and now and then , even when fresh putty is not laid on , the surface of the polisher should be touched with the brush to keep it moist .
When the polish of the metal nearly reaches the edge ( for it always , as I said before , begins in the middle ) you must alter your method of working ; for now the round strokes must be gradually altered for the short and straight ones .
Supposing then you are just beginning to alter them ; after having put on fresh putty , and gently rubbed it with two or three strokes of the bruiser , you place the metal on the tool , and after a stroke or two round and round , give it a few forward and backward , and from side to side , but with the edges very little over the tool ; then having turned the metal one-eighth round in your hand , and having moved yourself as much round the block ( which must be remembered throughout the whole process ) you go on again with a stroke or two round , to lead you only to the cross strokes , which are now to be principally used , and with more boldness .
After this has been done some time , the metal will begin to move stiffly as the friction now increases , and the speculum polishes very beautifully and fast ; and the whole surface of the polishing tool will be equally covered over with a fine metallic bronze .
The tool even now must not be suffered to become dry ; a single round stroke in each of your stations and turnings of the metal will be sufficient , and the rest must all be cross ones , for we are completing a circular figure .
You must now be very diligent , for the polisher drying , and the friction increasing very fast , the business of the spherical figure is nearly at an end .
As the metal wears much , its surface must be now and then cleaned , with a piece of shammy leather , from the black stuff which collects upon it ; and the polisher likewise from the same matter , with a soft piece of wet sponge .
You will now be able to judge of the perfect spherical figure of the metal and tool , when there is a perfect correspondence between the surfaces , by the fine equable feel there is in working , which is totally free from all jerks and inequalities .
Having proceeded thus far , you may put the last finishing to this figure of the metal by bold cross strokes , only three or four in the directions of each of the eight diameters , turning the metal at the same time : this must be done quickly , for it ought , in this part of the process particularly , to be remembered , that , if you permit the tool to grow quite dry , you will never be able , with all your force , to separate that and the metal , without destroying the polisher by heat .
The metal has now a beautiful polish and a true spherical figure , but will by no means make a sharp distinct image in the telescope : for the speculum ( if it be tried in the manner hereafter recommended ) will not be found to make parallel rays converge without great aberration ; indeed the deviation will be so great , as to be very sensibly perceived by a great indistinctness in the image .
How to give the parabolic figure to the metal .
In order then to give the speculum the last and finishing figure , which is done by a few strokes , it must be particularly remarked , that by working the metal round and round , the sphere of the polisher by this means growing less , it wears fastest in the middle : and as a segment of a sphere may become parabolic , by opening the extremes gradually from within outwards , so it may be equally well done by increasing the curvature in the middle , in a certain ratio , from without inwards .
Supposing then the metal to be now truly spherical , stop the hole in the polisher , by forcing a cork into it underneath , about an inch , so that it do not reach quite to the surface ; and having washed off any mud that may be on the surface of the tool with a wet soft piece of sponge , whilst the surface of it is a little moist , place the center of the metal upon the middle of the polisher ; then having , with the wet brush , lodged as much water round the edge of the metal as the projecting edge will hold , fill the hole of the metal and its handle with water , to prevent the evaporation of the moisture , and the consequent adhesion between the speculum and polisher , and let the whole rest in this state two or three hours : this will produce an intimate contact between the two , and by parting , with any degree of warmth they may have acquired by the vicinity of the operator , they will grow perfectly cold together .
By this time you may push out the cork from the polisher , to discharge the water , and give the metal the parabolic figure in the following manner .
Move the metal gently and slowly at first , a very little round the centre of the polisher ( indeed after this rest it will move stiffly ) then increasing by degrees the diameter of these strokes , and turning the metal frequently round its axis , give it a larger circular motion , and this without any pressure but its own weight , and holding it loosely between the fingers : this manner of working may safely be continued about two minutes , moving yourself as usual round the block , and carrying the round strokes in their increased and largest state , not more than will move the edge of the metal half an inch or five-eighths over the tool .
The speculum must not all this while be taken off from the polisher ; and consequently no fresh putty can be added .
It will not be safe to continue this motion longer than the time above-mentioned ; for if the parabolic tendency be carried the least too far , it will be impossible to recover a true figure of that kind but by going through the whole process for the spherical one in the manner before described , by the cross strokes upon the polisher , which takes a great deal of time .
However , when there is occasion , it may be done ; and I have myself several times recovered the circular figure , when I had inadvertently gone too far with the parabolic ; and ultimately finished the metal on the polisher without the use of the hones .
To try the true figure of the metal .
It will now be proper to try the figure of the speculum , and that is always best done by placing it in the telescope it is intended for .
In order to this , I use the instrument as a kind of microscope , placing the object , however , at such a distance that the rays may be nearly parallel .
At about twenty yards a watch-paper , or some such object , on which there are some very fine hair strokes of a graver , is fixed up .
The lead must be then taken off from the back of the speculum ; which is best done by placing the edge of a knife at the junction of the lead and metal , when , by striking the back of it with a flight blow , the pitch immediately separates , and the handle drops off ; the remaining pitch may be scraped off with a knife , taking care that none of the dust stick to the polished face of the metal .
Having placed the speculum in the cell of the tube , and directed the instrument to the object , make an annular kind of diaphragm with card-paper , so as to cover a circular portion of the middle part of the metal between the hole and the circumference , equal in breadth to about an eighth part of the diameter of the speculum : this paper ring should be fixed in the mouth of the telescope , and remain so during the whole experiment , for the part of the metal covered by it is supposed to be perfect , and therefore unemployed .
There must likewise be two other circular pieces of card-paper cut out , of such sizes , that one may cover the center of the metal by completely filling the hole in the last described annular piece ; and the other , such a round piece as shall exactly fit into the tube , and so broad as that the inner edge may just touch the outward circumference of the middle annular piece .
It would be convenient to have these two last pieces so fixed to an axis that they may be put in their places , or removed from thence so easily as not to displace or shake the instrument .
All these pieces therefore together will completely shut up the mouth of the telescope .
Let the round piece which covers the center of the metal , or that which has no hole in it , be removed ; and , by a nice adjustment of the screw , let the image ( which is now formed by the center of the mirror ) be made as sharp and distinct as possible .
This being done , every thing else remaining at rest , replace the central piece , and remove the outside annular one , by which means the circumference only of the speculum will be exposed , and the image now formed will be from the rays reflected from the outside of the metal .
If there be no occasion to move the screw and little metal , and the two images formed by these two portions of the metal be perfectly sharp and equally distinct , the speculum is perfect , and of the true parabolic curve ; or at least the errors of the great and little speculum , if there be any , are corrected by each other .
If , on the contrary , under the last circumstance , the image from the outside of the metal should not be distinct , and it should become necessary , in order to make it so , that the little speculum be brought nearer , it is plain that the metal is not yet brought to the parabolic figure ; but if , on the other hand , in order to procure distinctness , you be obliged to move the little speculum farther off , then the figure of the great speculum has been carried beyond the parabolic , and hath assumed an hyperbolic form .
When the latter is the case , the circular figure of the metal must be recovered ( after having fixed on the handle with soft pitch ) by bold cross strokes upon the polisher , finishing it again in the manner above described .
If the speculum be not yet brought to the parabolic form , it must cautiously have a few more round strokes upon the polisher ; indeed a very few of them in the manner before described make in effect a greater difference in the speculum than would be at first imagined .
If a metal of a true spherical figure were to be tried in the above mentioned manner in the telescope ( which I have frequently done ) the difference of the foci of the two segments of the metal would be so considerable , as to require two or three turns of the screw to adjust them ; so very great is the aberration of a spherical figure of the speculum , and so improper to procure that sharpness and precision so necessary to a good reflecting telescope .
This is by no means the case with the object glasses of refractors ; for besides that they are in fact never so distinct as well-finished reflectors , the apertures of them are so exceedingly small , compared to the latter , and the number of degrees employed so very small , that the inconvenience of a spherical figure is not so much perceived .
Accordingly we observe in the generality of reflectors ( whose specula , unless by accident , are always spherical ) that the only true rays which form the distinct image arise from the middle of the metal : and unless the defect be remedied by a considerable aperture , which destroys much light , the false reflection from the inside of the metal produces a greyish kind of haziness , which is never seen in Mr. SHORT'S or indeed in any good telescopes .
Supposing that the two foci of the different parts of the metal perfectly coincide , and that , by the union of them when the apertures are removed , the telescope shows the objects very sharp and distinct , you are not however even then to conclude that the instrument is not capable of farther improvement ; for you will perceive a sensible difference in the sharpness of the image , under different positions of the great speculum with respect to the little one , by turning round the great metal in its cell , and opposing different parts of it to different parts of the little metal , correcting by this means the error of one by the other .
This attempt should be persevered in for some time , turning round the great speculum about one-sixteenth at a time , and carefully observing the most distinct situation each time the eye-piece is screwed on : when , by trying and turning the great metal all round , the distinctest position is discovered , the upper part of the metal should be marked with a black stroke , in order that it may always be lodged in the cell in the same position .
This is the method Mr. SHORT always used ; and the caution is of so much consequence , that he thought it necessary to mention it very particularly in his printed directions for the use of the instrument .
And farther , Mr. SHORT frequently corrected the errors of the great by the little metal in another way .
If the great speculum did not answer quite well in the telescope , he cured that defect sometimes by trying the effect of several metals successively , by this means correcting the errors of one by the other ; for in several of his telescopes which have passed through my hands , when the sizes and powers have been the same , I have found that the great metals , though very distinct in their proper telescopes , yet have , when taken out and changed from one to the other , spoiled both telescopes , rendering them exceedingly indistinct , which could arise from no other circumstance .
For this reason I suppose it was , that he kept , ready finished , a great many large metals of the same focal length , so that , when he wanted to mount a telescope , he might from a great choice , be able to combine those metals which suited each other best .
I am strongly inclined to believe this was the case , not only from the above observation , but because he showed me himself a box of finished metals , in which I am sure there were a dozen and a half of the same focal length .
To return : a little use in working will make the whole of the process of grinding and polishing very easy and certain ; for though I have endeavoured to be as particular as I can ( I am almost afraid too much so ) it is yet scarcely possible to supply a want of dexterity , arising from habit only , by the most laboured and minute description .
And though the above account may appear irksome to the reader , as it lies cold before the eye , I am very sure , whoever attempts to make the instrument , will not complain of it as tediously particular .
I will , however , farther remark , that when the metal begins to move stiffly upon the polisher , and particularly when the figure is almost brought to the parabolic form , it will be necessary to fix the elbows against the sides , in order to give momentum and equability to the motion of the hand by that of the whole body .
The same polisher will serve for several metals , if it be somewhat warmed when you begin to use it .
There is another circumstance , and a material one too , which must not be omitted ; it is this .
For the very same reason that the pitch should not be too hard or soft , the work will not proceed well in the heat of summer , or the cold of winter : in the latter , it may be possible to remedy the defect by having the room warmed with a stove ; and in the summer , the other inconvenience may perhaps be avoided by using a harder kind of pitch ; but I much doubt in either case whether the work will go on so kindly : I have myself always wrought in spring and autumn .
The process of polishing , and indeed grinding upon the hones , will not go on so well if it be not continued uninterruptedly from beginning to end ; for if the work of either kind be left but for a quarter of an hour , and you then return to it again , it will be some time before the tool and metal can get into a kindly way of working ; and till they do , you are hurting what was done before .
I have all along supposed that the metal we have been working was about four inches diameter : if it be either larger or smaller , the sizes of the hones , bruiser , and polisher , must be proportionably different .
I never find any ill consequence arising from the different expansion from heat and cold in any of the tools , though they be made of different metals and substances , unless the inconvenience , occasioned by the interruption before hinted at , bethought to result from thence ; for the alteration produced in the surface of the speculum , both by grinding and polishing , is so much quicker than any that can be supposed to arise from the former cause , that it is never attended with any practical consequence .
Magnifying very minute objects , and particularly reading at a distance , have been generally considered as the surest tests of the goodness of a telescope ; and indeed when the page is placed at a great distance , so that the letters subtend but a very small angle at the eye , if then they appear with great precision and sharpness , it is most probable that the instrument is a good one .
But we are , nevertheless , sometimes apt to be deceived by this method ; nor is it always possible to determine upon the different merits of two instruments of equal power , by this mode of examination ; for when the letters are removed to the utmost extent of the powers of the two instruments , the eye is apt to be prejudiced by the imagination .
If two or three words can be here and there made out , all the rest are guessed at by the sense ; insomuch that an observer , zealous for the honour of his instrument , is very apt to deceive himself in spite of his intentions .
The surer test is by figures , where you can procure no aid from this sort of deception .
In order to examine my reflecting telescopes , I made upon a piece of copper and on a black ground , six lines consisting of about twelve pieces of gold figures , and each line of figures differing in magnitude , from the smallest that could be distinctly made to those of about two-tenths of an inch long ; moreover , the figures in the several lines were differently disposed , and the sum of each line also differed .
It is evident that by this method all guess is precluded ; and that of two instruments , of the same powers , that which can make out the least order of figures , which will be known by the sum , is the best telescope .
Such a plate I caused to be fixed up for experiments against the top of a steeple , about three hundred yards North of my house ; and it will serve to give some idea of the distinctness with which very small figures could be made out at that distance , by saying , that in a clear state of the air , and with the Sun behind me , with a telescope of eighteen inches focal length , which Count BRUHL did me the honour to accept and now has in his possession , I have seen the legs of a small fly , and the shadows of them , with great precision and exactness .
I cannot conclude without indulging myself in an observation on the amazing sagacity of Sir ISAAC NEWTON in every subject upon which he thought fit to employ his attention .
It was he who first proposed , and indeed practised , the polishing with pitch ; a substance which at first sight perhaps every one but himself would have thought very improper , from its softness , to produce that correctness of figure so necessary upon these occasions ; and yet I do believe , that it is the only substance in nature that is perfectly well calculated for the purpose ; for at the same time that it is soft enough to suffer the putty to lodge very freely on its surface , and for that reason to give a most tender and delicate polish ; it is likewise totally inelastic , and therefore never , from that principle , suffers any alteration in the figure you give it .
If the first makers of the instrument , therefore , had given proper credit to , or had simply followed the hint Sir ISAAC gave , it would have saved them infinite trouble , and they would have produced much better instruments ; but the pretended refinement , of drawing a tincture from pitch with spirits of wine , affords you only the resinous , hard , and untractable part of the pitch , divested of all that part of its original substance which is necessary to give it that accommodating pliability in which its excellence consists .
It is needless to swell this account with a detail of the process for polishing the little speculum , as it must be conducted in the same manner which has been already described in that of the large one ; only observing , that as the little metal has an uninterrupted face , without a hole , so there is no occasion for one in the polisher ; and likewise that , as a spherical figure is all that need here be practically attempted , so the difficulty in finishing is infinitely short of that of the other .
As it is always necessary to folder to the back of the little speculum a piece of brass , as a fixture for the screw to adjust its axis , I shall just hint a safe and neat method of doing it , which may be very useful to the optical or mathematical instrument-maker upon other occasions .
Having cleaned the parts to be soldered very well , cut out a piece of tin-foil the exact size of them ; then dip a feather into a pretty strong solution of sal ammoniac in water , and rub it over the surfaces to be soldered ; after which place the tin-foil between them as fast as you can ( for the air will quickly corrode their surfaces so as to prevent the solder taking ) and give the whole a gradual and sufficient heat to melt the tin .
If the joints to be soldered have been made very flat , they will not be thicker than a hair : though the surfaces be ever so extensive , the soldering may be conducted in the same manner , only that care must be taken , by general pressure , to keep them close together .
In this manner , for instance , a silver graduated plate may be soldered on to the brass limb of a quadrant , so as not to be discernable by any thing but the different colour of the metals .
This method was communicated to me by the late Mr. JACKSON , who during his life kept it a secret , as he used it in the construction of his quadrants , and is , I believe , not as yet known to any workman .
In the annexed plate are figured the shape of the leaden tool for rough-grinding ; the hones ; and the apparatus to be applied to the mouth of the telescope , to ascertain the true figure of the speculum .
POSTSCRIP T. It was some time after I had written the above account that I saw Mr. SHORT'S method of polishing object glasses for refracting telescopes , which is published in the Transactions .
By that paper I find that what I before strongly suspected is really the case , viz. that he knew how well pitch was calculated for purposes of this kind .
Only it may be remarked , that as glass is much harder , polishes much slower , and consequently does not wear away and alter its figure so soon as the metal of which the speculum is made ; and as at the same time ( on account of the very small apertures allowed to telescopes of this sort ) nothing more than a spherical figure is proposed ; he is therefore obliged to use pitch in a hard , friable , and stubborn state : whereas , considering the delicate substance of the metal speculum , and the figure intended to be given to it , the soft pitch of the common sort , by suffering the putty to bed itself in its substance , produces the most beautiful polish ; and by its pliability is better calculated for that mutual accommodation between polisher and metal , so necessary to the figure proposed .
EXPLANATIONOFTHEFIGURE S. Fig. 1 .
The grinder for working off the rough face of the metal ; the black strokes represent deep grooves made with a graver .
Fig. 2 .
The bed of hones , which is to complete the spherical figure of the speculum , and to render its surface fit for the polisher .
Fig. 3 .
An apparatus for examining the parabolic figure of the speculum .
AA The mouth of the telescope , or edge of the great tube .
BBA thin piece of wood fastened into , and flush with the end of the tube ; to which is permanently fixed the annular piece of paste-board CC , intended to cover , and to prevent the action of the corresponding part of the speculum .
Fig.1 st. Fig.2 d. B H ACA H CG Fig.3d .
G E B FD F D Another piece of paste-board , fixed by a pin to the piece of wood BB , on which it turns as on a center ; so that the great annular opening HH may be shut up by the ring FF , or the aperture GG by the imperforate piece E in such manner that , in the first instance , the reflexion may be from the center , and in the latter from the circumference , of the great speculum .