III .
The Method of making Tin-Plates , extracted from the Memoirs of the Academy of Sciences , for the Year 1725 , by William Rutty , M. D. R. S. Secr. THE making of Tin-plates , or Latin , as it is called , being not commonly practised in England , though there is so great a Consumption of it , either because the Method is not sufficiently known , or because that in Use to make small Quantities for particular Purposes is much too dear to answer the Artificer 's Expectation in making larger , whereby we are obliged to export our own Tin to Germany , to receive it back again manufactured , I thought it not improper to lay before the Society the Method the Germans themselves make use of , as I have extracted it from a Dissertation of Mr. De Reaumur , printed in the last Volume of the Memoirs of the Academy of Sciences of Paris , in which also he lays down some Improvements , as he thinks , of his own .
He takes notice then that the making of Tin-plates , ( which is called in France , white Iron ) does not properly begin , till they go about to prepare the Leaves or Plates of Iron that are to be tinned , which are supposed to be sufficiently thin and flat , and cut into Squares : But there are only certain Sorts of Iron which can be reduced into these Leaves , of which those are the most proper , that when heated are easiest extendible , and yet can be forged with a Hammer when cold ; the more soft and extremely flexible , as well as the more brittle being to be rejected .
These Leaves are drawn from Bars of Iron , about an Inch square ; which being made a little flat , they cut into thin Pieces or Soles ( semelles ) which they fold together , and having made them into Parcels containing forty Leaves each , beat them all at once with a Hammer that weighs from 600 to 700 ~ .
Weight .
After this , the principal Part of the whole Art is to prepare these Leaves ; for the lightest Dust , or the least Rust upon their Surface will prevent the Tin from uniting with them .
This may indeed be taken off by filing , but that being much too expensive , the same may be brought about by steeping the Plates in acid Waters , for a certain Time , to what Number they please , and when they are taken out , scouring them with Sand , in order to fetch off any Thing that may remain upon the Surface : And by this Method a Woman may clean more Plates in an Hour , than the most expeditious Workman can file in many Days .
Of these Waters the Author mentions several ; but what the Germans themselves used , and which they make a mighty Secret of , he found to be only common Water made eager with Rye , which requires very little Pains .
For after they have ground the Grain grossly , and pounded it , they leave it to ferment in common Water for a certain Time , and with a little Patience they are sure to have an eager Menstruum .
With this Menstruum they fill Troughs or Tuns , into which they put Piles of Iron Plates ; and to make it grow eager the better , and to have more Activity , they keep these Vessels in Vaults or Stoves which have little Air , and in which they keep lighted Charcoal .
The Workmen go into these Vaults once or twice in a Day , either to turn the Plates that they may be equally exposed to the Action of the acid Liquor , or to take out those that are sufficiently cleansed , or to put others in their room : And as the Liquor is more acid , or the Heat of the Vault or Stove is more intense , the Plates are sooner cleansed ; but it requires at least two Days , and sometimes a great deal more .
This is the Method which the Cermans employed in the Tin-works in France , constantly made use of to prepare the Iron-plates to receive the Coat of Tin : But as the Author observed , that the constant Attendance upon them in the Stoves was very laborious , the Heat therein being almost insupportable to those who are not used to it , he proposes some other Methods which are attended with very little Trouble , and as small , if not a less Expense ; and which upon Trial succeeded full as well .
Having therefore observed that the Iron-leaves or Plates are covered with a Scale or Layer , half vitrified by the Fire , on which Acids have none or very little Effect~ he imagined that instead of dissolving the Iron in these acid Waters , it would be better to make it rust , and thereby put it in a Condition to be easier cleansed from these Scales ; as Rust is accompanied with a sort of Fermentation and Rarefaction , and the Matter which rusts takes up a greater Space , and raises up whatever opposes it .
To this Purpose he steeped Iron Plates in different eager Menstruums , as in Water in which Alum , common Salt and Sal-armoniack were separately dissolved ; and others of the same Iron he only dipped into the same Waters , and instantly taking them out exposed them to the Air .
These latter were rusted by all of them , but sooner by that in which the Sal-armoniack was dissolved .
After two Days , during which every Plate had been dipped ped into the Menstruum but twice or thrice , he scoured them , and likewise those he had left to steep for that Time ; and comparing them together , found that those , which had been only wetted at different Times , cleansed better than those which were steeped ; the Rust covering all the Surface of the latter without raising the Scale ; whereas in the former , as soon as one Part of the Metal is detached , it is attracted by the Menstruum , and the Surface is raised into Blisters of Rust .
These Dissolvents , the Author takes notice , tho ' weak in themselves , yet produce the Effect as well as the stronger , which are much dearer : But amongst the latter he prefers Vinegar , which being very plentiful in France , may be used with little Cost .
For you need only dip each Leaf into it , and take it out again immediately , leaving it afterwards in some moist Place , and it will be scaled in eight and forty Hours , if you take care to repeat this 3 or 4 Times in a Day .
The scaling will still be more expeditious , if you dissolve a little Sal-armoniack in the Vinegar , a Pound or two to a Puncheon ; for as the Vinegar dissolves Iron well , so Sal-armoniack , as just observed , rusts it sooner than any other Salt : But this must be used very moderately , and the Leaf must be left to steep in clean Water to dissolve any Particles of it that may stick to its Surface , which may otherwise make it rust after it is tinned .
If you scale with Vinegar , and want to do it at a less Expense , you need only plunge the Leaves once or twice at farthest , and when the Vinegar is dried upon the Surface , sprinkle it with Water ; or dip them into it , and take them out immediately .
There are several other Ways of making Iron rust , as keeping it in a moist Cellar , exposing it to the Dew , sprinkling it with simple Water , several Times in a Day , which will still act quicker by dissolving Sal-armoniack in it .
In those Countries where the Pyrites is common , the Vitriolick Waters will scale them soon enough , which are almost as cheap as common Water : You need only heap the Pyrites together , and leaving them to moulder in the Air , make afterwards a Lixivium with them and common Water , which Lie will have the desired Effect : But as the Leaves of Iron are sensibly much easier cleansed on one Side than the other , the bad Side rarely taking the brilliant Polish in the tinning , but having always some Spots , which proceeds in that in the beating one Side is more exposed to the Action of the Hammer , and is therefore better plained , the Author again advises not to steep them , but only to moisten them , in order to make them rust , whereby you need moisten that Side only that wants it most : Whereas if you steep them , as the bad Side will take double or triple the Time of the other , the acid Menstruum will dissolve the Surface , and occasion a Loss of Iron .
He next gives two Cautions necessary to be followed : the first is in the Management of the Plates before they come to be prepared ; which is in the beating of them , to change the Place of each in its Turn , that every one may receive the immediate Action of the Hammer , otherwise they will not extend equally : the second is to steep them in Clay or Fuller 's earth tempered with Water before you heat them , to prevent their soldering with one another .
He then closes this Part of the Operation with remarking that whatsoever of these Methods are pitched upon , whether the old one , of which he has learnt the Secret , or any of the new , which he has here shown , it is absolutely necessary after the Plates are sufficiently scaled , to scour them with Sand , and when there remains no more black Spots upon their Surface , to throw them into Water to prevent their rusting again , and leave them in it till the Instant you would tin them , or in the Term of Art , blanch them .
This he observes is the very Object of the whole Art , and is kept as much a Secret by the Blancher , as the acid eroding Menstruum is by the Scaler : But the Manner of doing it is thus .
They flux the Tin in a large iron Crucible , which has the Figure of a broken Pyramid with four Faces , of which the two opposite ones are less than the two others .
This Crucible they heat only from below , its upper Border being luted in the Furnace quite round .
The Crucible is always deeper than the Plates which are to be tinned are long , which they always put in downright , and the Tin ought to swim over them .
For this Purpose Artificers of differrent Trades prepare the Plates in different Manners , which are all exceptionable : But the Germans he perceived made use of no Preparation whatsoever , except putting the scoured Plates into clean Water , as just remarked ; but when the Tin is melted in the Crucible , they cover it with a Layer of a Sort of Suet , an Inch or two thick , through which the Plate must pass before it comes to the Tin : The first Use of which is to keep the Tin from burning , and if any Part should take Fire , as the Suet will soon moisten it , to reduce it to its natural State again .
This Suet is compounded , as the Blanchers say , and is of a black Colour , which the Author thought might be given it with Soot or the Smoke of a Chimney , only to spread a Mystery over their Work ~ but he found it true so far , that common unprepared Suet was not sufficient : For after several Attempts , there was always something wanting to render the Success of the Operation certain .
The whole Secret then of Blanching lies entirely in the Preparation of this Suet : And this he at last discovered to consist only in first frying and burning it ; which not only gives it the Colour , but puts it into a Condition to give the Iron a Disposition to be tinned , which it does surprisingly .
The Tin itself ought to have a certain Degree of Heat ; for if it is not hot enough it will not stick to the Iron ; if it is too hot , it will cover it with too thin a Coat , and the Plates will have several Colours , as a Mixture of red , blue , and yellow , and the whole appear of a villainous yellow Cast .
To prevent this , by knowing when the Tin has a proper Degree of Heat , they might first make an Essay with small Pieces of the scaled Plates , and they would learn from them when the Tin is in proper Order : But generally speaking , they dip the Plates into Tin that is more or less hot , according to the Thickness they would have the Coat to be of .
Some Plates they only give one Layer to , and these they plunge into Tin , that has a lesser Degree of Heat than that into which they plunge those Plates which they would have take two Layers ; as also when they give these the second Layer , they put them into Tin that has not so great a Degree of Heat , as that into which they were put the first Time : Besides which , it is to be observed , that the Tin , which is to give the second Coat , ought to be fresh covered with Suet , but only with the common Sort without Preparation ; for melted Tin is sufficiently disposed to attach it self to solid Tin ; and in this Case it is to tin itself , to which the new Tin is to be joined .
As to the Choice of the Tin , the Manner of making it is as bright as possible , with a Number ber of little Articles necessary to the Practice , the Author refers them to another Time , as more properly belonging to the Description of the whole Art , than to a Memoir in which he only gives the Principles of it .