The Art of Refining , communicated by Dr. Christopher Merit .
THe end hereof , is the separation of all other Bodies from Gold and Silver ; which is performed four ways , viz. By Parting , by the Test , by the Almond Furnace or the Sweep , and by Mercury .
PARTING is done with Aqua fortis , which the Refiners make thus , ~ Salt Peter ~ iii .
Dantzick Vitriol ~ ii .
Let them be well bruised and mixed in a Mortar and then put into a Long neck , which is an Earthern Vessel so named from its Figure .
Then six or eight of these Long necks thus filled , are placed in each side of their Furnace , on a Range built with Iron Bars , of the form of a parabola , at above nine Inches distance one from another , and closed at the sides with Bricks .
The upper Arches are left open to put in and take out the Pots .
Over the said Arches they lay large Bars of Iron , and then cover all the top of the Furnace with Lome , the Body of each Long-neck lying naked to the Fire , the Neck outward ; to which the Receivers , whether of Glass or German Pots , are well Luted .
Note that if the Vitriol be not Dantzick , which is made with Copper ; but English , wheh is made with ~ Iron ; the Water will be weaker , and make a dirty coloured Verditer , and wholly spoil it ; besides , the Silver will not gather so well to the Copper after dissolution , and thereby becomes black .
Their Lute is made of good Lome , some Horse Dung , and a little Colcothar ; although the two former do well .
The luting being well laboured and applied , they make a gentle Charcoal fire under the Pots , for three hours , and then increase it for three hours more : about the seventh hour , they make a vehement hot Fire for four hours , and cast in at last well dried Billets of the length of the Furnace , whose flame surroundeth all the Pots , and finishes therir Work .
The next morning they carefully separate the Receivers from the Long-necks .
Usually performing this Work but once in 24 .
hours , sometimes twice .
Some Refiners distill 100 lb of the materials put into a CastIron-Pot ; which is the best way , especially being perfomed after this latest Invention , viz. Build a Furnace two yards high or more ; and at the top place in your Iron-Pot .
To which fit a Head of Earth , like the Head of a large Distillatory for Chemical Oils , which must have a large belly , branching it self , about eight inches from the Iron Pot , into three Branches : one whereof in the midst , comes directly straight forwards , two other lateral ones obliquely : all which Branches are four or five Inches hollow in diameter , and fiveor six long .
To these Branches are fitted Glass Bodies , narrow and hollow at both ends , large and globous in the midst .
These must be exceedingly well luted on with Colcothar , Rags , Flower and Whites of Eggs .
To this first Glass-Body is luted on another Glass , of the same figure and size , and in order eight alike in all , till they come to the Receiver , which is an ordinary Gallon Glass .
All these Rows of Glasses lye on boards ~ from the Head to the Receiver .
The two upper Receivers or Glass-Bodies need exceeding good Luting , for the rest ordinary Lute will serve .
The convenience of this way is , that a little Fire , and that of New Castle-Coals , will do the work , you save a Longneck for each five pounds of materials , and you need never break or un'ute any of the Receivers , but the lowermost .
The Aqua fortis being distilled off , is put into a large Earthen Pot , and there is added of fine Silver , one or two penny weight ( which is called Fixes ) to every pound of Aqua sortis , which within four hours will purge it from all dirt and impurity , and make it fit for Parting , which is thus done .
If their Silver guilt be fine enough for Wire they only melt it in a Wind-furnace , and cast it melted into a large Tub of water , that they may have it in small pieces .
But if it be but standard , they first fine it on the Test .
These small pieces taken from the water , being well dried , are put into a Glass taperfashion , fashion , a foot high , and seven inches at the bottom ; and then the Glasses are charged with Aqua fortis about two thirds of it , and set in a Range of Iron-covered two inches deep with Sand , and a gentle Charcoal fire made under it .
Small bubles will-soon arise , and the water also run over .
If so , they take off the Glasses , and hold them , till it doth deservescere , or else pour some of it into a Vessel which isat hand .
If Lead be mixed with it , they cannot keep it from running over .
When the Water hath oncebeen quieted , from this Ebullition , it will rise no more .
The greenness of the Water , manifesteth the quantity of Copper contained in it .
If the water boil over , 'twill penetrate the Bricks and Wood .
They commonly let it stand a night on the Iron Range , with a gentle heat under it , and in the morning softly pour off the water impregnated with all the Silver ; all the Gold lying , like black dirt , at the bottom , which being washed out is put into small Parting-Glasses , and set over the Sand with fair Conduit-water for an hour , and then the water poured off .
This is repeated five or six times , to seperate the Salt from the Gold , which is now fit to be melted , and Cast into an Ingot .
To regain the Silver they have large round Washing .
Bowls , lined within with melted Rosin and Pitch ( for otherwise the Water would eat the Wood and penetrate the sides of the Bowl ) covered with Copper Plates ten inches long , six wide , and half or more thick .
Into which Bowles they pour good store of water ( the more , the better the Verditer ) and then the Silver-water : which working on the softer Metal of Copper , leaves all the Silver in most fine Sand at the bottom , and sides of the Bowl and Plates of Copper ; which being taken out , is washed , dried and melted for any use .
Concerning the Plates it is observable , That if any Brass or shroffe Metal be in them ; they gather very little of the Silver , the latter mixing with the Silver , as it was proved at the Tower by a Finer questioned for his Silver .
With the Copper-Water poured off from the Silver , and Whiting , Verditer is made thus .
They put into a Tub a hundred pound weight of Whiting , and thereon pour the Copper-Water , and stir them together every day , for some hours together .
And when the Water grows pale , they take it out , and set it by for further use , and pour on more of the Green-Water , and so continue till the Verdter be made .
Which being taken out , is laid on large pieces of Chalk in the Sun , till it be dry for the Market .
The Water mention to be taken from the Verditer , is put into a Copper , and boiled till it comes to the thickness of Water gruel , now principally consisting of Salt Petre reduced ( most of the Spirit of Vitriol being gone with the Copper into the Verditer .
) A dish full whereof being put into the other Materials , for Aqua fortis , is redistill 'd , and makes a double-water , almost twice as good , as that without it , and sold for near a double value .
1 COME next to the second way of Refining , sc .
by the TEST .
This seperates all Metals from Silver , except Gold , because they swim over it , when they are all melted together .
The Test is thus made .
They have an Iron Mould , oval , and two inches deep .
At the bottom hereof , are three Arches of Iron set at equal distances , two fingers wide , if the great diameter of it be fourteen inches long ; and so proportionably in greater or lesser Tests .
This cavity they fill with fine powder of Bone-ashes moistned with Lixivium made with Soap-ashes .
Some use Cakes of Pot ashes or other Ashes well cleansed , and so pressed well together with a Muller , that it becomes very close and smooth at the top .
There is left above a Cavity in the midst of it , to contain the melted Silver .
This Cavity is made greatest in the middle ; for the Bone-Ashes come up parallel to the circumference of the Mould ; only a small Channel in that end , which is most remote from the blast , for the running off of the baser Metals , and so is made declive to the centre of the Test , where it is not above half an inch deep .
The Test thus made , is set annealing 24 .
hours , and then it is fit for use , in this manner .
It is set in a Chimney a yard high , parallel almost to the Nose of a great pair of Bellows , and then therein is put the Silver .
Which being covered all over with Billets of barqued Oak , the blast begins and continues all the while strongly .
The Lead purified from all Silver , ( which they call the Soap of Metals ) first put in , melts down with the Silver , and then the Lead and Copper swim at the top , and run over the Test .
Whose motion the Finer helps with a long Rod of Iron drawn along the surface of the Silver towards the forementioned slit , and often stirring all the Metal , that the impurer may the better rise : and by continuing this course , separation is made in two or three hours .
The greatest part of the Lead flies away in smoke .
If the Lead be gone before all the Copper , 'twill rise in small red fiery bubbles ; and then they say , the Metal Drives , and must add more Lead .
The force of the blast drives the higher Metals to the lower side of the Test , and helps its runing over .
When the Silver is fully fined , it looks like most pure Quicksilver ; and then they take off their sogs and let it cool .
In the cooling , the Silver will frequently from the middle spring up in small Rays and fall down again .
If moist Silver be put into that which is melted , 'twill spring into the fire .
A good Test will serve two or three firings .
So soon as the Silver will hold together , they take it out of the Test , and beat it on an Anvil into a round figure , for the Melting Pot : which being set in a Wind-Furnace , surrounded with Coal , and covered with an Iron Cap , that no Charcoal fall into it , is then melted .
If any Dross or filth be in the Melting-Pot , they throw in some Tincal , which gathers the dross together that it may be separated from it .
These Melting-Pots are never burned , but only dried , and will last a whole day , if they be not suffered to cool : but if they once cool , they infallibly crack .
NEXT IS the ALMOND-FURNACE or Sweep .
Here are separated all sorts of Metals from Cinders , parts of Meling-Pots , Tests , Brick , and all other harder bodies ; which must be first beaten into small pieces with a hammer , and an Iron Plate ; and it is one mans work .
Those which stick but superficially to their Silver , they wash off thus ; they have a Wooden round Instrument two foot wide , somewhat hollow in the middle , with a handle on each side .
On this they put the Materials , and hold them in a Tub of Water below the surface , and so waving it to and fro , all the lighter and looser matter is separated from the Metal .
The Furnace is six feet high , four feet wide , and two feet thick .
Made of Brick ; having a hole in the midst of the top eight inches over , growing narrower towards the bottom of it , where , on the fore part , it ends in a small hole , environed with a semicircle of Iron to keep the molten Metal .
About the middle of the Back , there is another hole to receive the Nose of a great pair of Bellows , requiring continually the strength of two lusty men .
The night before they begin , Charcoal is kindled in the Furnace to Anneal it : and when it is hot , they throw two or three shovels of Coal , to one of the forementioned Stuff , and so proceed during the whole Work , making stratum super stratum of one and the other .
After eight or ten hours the Metal begins to run ; and when the Receiver below is pretty full , they lade it out with an Iron Ladle , and cast it into Sows in Cavities or Forms made with Ashes .
They frequently stop the passage-hole with Cinders to keep in the heat ; and when they think a quantity of Metal is melted , they unstop the hole to pass it off .
If the Stuff be hard to flux , they throw in some slag ( which is the Recrement of Iron ) to give it fusion .
Their Irons melt away apace , wherewith they proak out the Cinders from the hole .
A stinking blue smoke proceeds from the Furnace , and all by-standers put on the colour of dead men .
The workmen must be well lined with Oil , Sack , Strong Beer , and good Victuals : for the Work continues three days and nights without intermission , using no other variety , than above said .
A large Cavity will be made in the Furnace : for the Metals or the Fire , or both together corrode and wear the greatest part of the bricks away .
To get the Silver from these Metals , they now use no other Art , than that of the Test .
To Refine their Copper from the Litharge , they formerly laid their Ingots of Lead and Copper on Loggs of Wood fired , which would easily melt down the Lead or Tinn , and so leave the Copper full of holes wherein the Lead had been lodged .
But now they commit this work also to the Test .
THE LAST way of Separation is by Quick-silver .
And this is for filings of small Workers and Goldsmiths , wherein Gold and Silver are mixed with dust , &amp;c. This dust is put into a Hand-mill with Quick-silver , and being continually turned upon that , and the Metals , an Amalgama is made of them , and fair water poured in , carrys off the dust as it runs out again by a small Quill .
This Amalgama is put into an Iron with a Bolt Head , set into the fire , having a long Iron-neck three feet long , to which is fitted a Receiver .
The fire distils off the Mercury into the Receiver , and the Gold and Silver remain in the Bolt Head .